MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Arkema KYNAR® 6000 HD Polyvinylidene Fluoride - Injection Molding
Categories: Polymer; Thermoplastic; Fluoropolymer; Polyvinylidene Fluoride (PVDF); Polyvinylidinefluoride (PVDF), Molded/Extruded

Material Notes: Characteristics: Natural resin - translucent, off-white hemispheres. High stability in harsh thermal, chemical and ultraviolet environments. High toughness and mechanical strength, low permeability, abrasion resistance; high purity

Applications:

  • Chemical processing – production, storage and transfer of corrosive fluids
  • Electronics – protective sheathing, plenum and wiring insulation
  • Semi-conductor industry
  • Food stuff and Healthcare industries
  • Transportation – fuel line and pipe, thermoformed body components

Information provided by Arkema Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.77 g/cc0.0639 lb/in³ISO 1183
Water Absorption 0.020 %0.020 %Dry; Sim. to ISO 62
Moisture Absorption 0.0150 %0.0150 %Dry; Sim. to ISO 62
Viscosity 110000 cP
@Shear Rate 100 1/s,
Temperature 230 °C
110000 cP
@Shear Rate 100 1/s,
Temperature 446 °F
Melt; ASTM D3835
Linear Mold Shrinkage, Flow 0.020 cm/cm0.020 in/inDry; ISO 294-4, 2577
 0.020 cm/cm0.020 in/in
Melt Flow 6.7 g/10 min
@Load 5.00 kg,
Temperature 230 °C
6.7 g/10 min
@Load 11.0 lb,
Temperature 446 °F
cm³/10 min Volumetric Rate; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 52.0 MPa7540 psiDry; ISO 527-1/-2
Elongation at Break 40 %40 %Dry; ISO 527-1/-2
Elongation at Yield 9.0 %9.0 %Dry; ISO 527-1/-2
Tensile Modulus 2.30 GPa334 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  22.1 J/cm²
@Temperature -30.0 °C
105 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eU
 22.7 J/cm²
@Temperature 23.0 °C
108 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eU
Charpy Impact, Notched  0.500 J/cm²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 1.20 J/cm²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+12 ohm-cm1.00e+12 ohm-cmDry; IEC 60093
Surface Resistance 1.50e+14 ohm1.50e+14 ohmCond.; IEC 60093
Dielectric Constant  7.0
@Frequency 1e+6 Hz
7.0
@Frequency 1e+6 Hz
Dry; IEC 60250
 9.5
@Frequency 100 Hz
9.5
@Frequency 100 Hz
Dry; IEC 60250
Dielectric Strength 24.0 kV/mm610 kV/inDry; IEC 60243-1
Dissipation Factor  0.028
@Frequency 100 Hz
0.028
@Frequency 100 Hz
Dry; IEC 60250
 0.22
@Frequency 1e+6 Hz
0.22
@Frequency 1e+6 Hz
Dry; IEC 60250
Comparative Tracking Index 600 V600 VDry; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 150 µm/m-°C83.3 µin/in-°FDry; ISO 11359-1/-2
Melting Point 171 °C340 °F10°C/min; Dry; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 108 °C226 °FDry; ISO 75-1/-2
Vicat Softening Point 140 °C284 °F50°C/h 50N; Dry; ISO 306
Glass Transition Temp, Tg -40.0 °C-40.0 °F10°C/min; Dry; ISO 11357-1/-2
Flammability, UL94  V-0
@Thickness 0.800 mm
V-0
@Thickness 0.0315 in
IEC 60695-11-10
 V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
IEC 60695-11-10
Oxygen Index 80 %80 %ASTM D2863
 80 %80 %Dry; ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 220 °C428 °FInjection Molding; ISO 294
Mold Temperature 90.0 °C194 °FInjection Molding; ISO 10724
Injection Velocity 10.0 mm/sec0.394 in/secInjection Molding; ISO 294
Hold Pressure 13.0 MPa1890 psiInjection Molding; ISO 294
 
Descriptive Properties
Form as DeliveredGranules
Heat StabilizedYes
Light StabilizedYes
Moisture SensitiveNo
Processing MethodsCasting
 Film Extrusion
 Injection Molding
 Profile Extrusion
 Sheet Extrusion
 Thermoforming

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Arkema Kynar® 710 Polyvinylidene Fluoride Homopolymer- Injection Molding
Arkema KYNAR® 370 Polyvinylidene Fluoride (PVDF) Homopolymer - Injection Molding
Arkema KYNAR® 9000 HD Polyvinylidene Fluoride - Injection Molding
Arkema KYNAR® 1000 HD Polyvinylidene Fluoride Homopolymer - Injection Molding and Extrusion
Arkema KYNAR® 761 Polyvinylidene Fluoride Powder

PARKG911 / 144536

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.