MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Elkem (Bluestar Silicones) BLUESIL™ RTV 3625 Hi-Pro Green Silicone Rubber
Categories: Polymer; Thermoset; Silicone; Silicone Rubber

Material Notes: Description: BLUESIL™ RTV 3625 is a low viscosity, 25 Durometer (Shore A), two component, tin catalyzed, room temperature curing silicone elastomer. It is designed as a high strength elastomer with good cured rubber properties, long library life and accurate detail reproduction. BLUESIL™ RTV 3625 can be catalyzed with BLUESIL™ Hi-Pro Green or fast setting BLUESIL ™ Hi-Pro Blue.

Applications:

  • Casting of polyester or polyurethane resins for figurine, giftware and decorative accessories
  • Architectural and furniture parts and accessories
  • Statuary and collectibles

Information provided by Bluestar Silicones

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.11 g/cc1.11 g/cc
Viscosity 90 cP90 cPPart B, Catalyst Component
 30000 cP30000 cPMixed
 40000 cP40000 cPPart A, Base Component
Linear Mold Shrinkage  0.0020 cm/cm
@Time 86400 sec
0.0020 in/in
@Time 24.0 hour
 0.0040 cm/cm
@Time 25200 sec
0.0040 in/in
@Time 7.00 hour
Storage Temperature 24.0 °C75.2 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 2323ASTM D2240
 252524 hr thick section
Tensile Strength 4.55 MPa660 psiASTM D412
Elongation at Break 450 %450 %ASTM D412
Tear Strength 21.9 kN/m125 pliASTM D624, Die B
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 150 °C302 °F
Minimum Service Temperature, Air -50.0 °C-58.0 °F
 
Processing PropertiesMetricEnglishComments
Cure Time 10100 min
@Temperature 24.0 °C
168 hour
@Temperature 75.2 °F
50% RH
Pot Life 240 min240 min
Working Life 960 min960 min
Shelf Life 18.0 Month18.0 Month
 
Descriptive Properties
ColorLt. GreenPart B, Catalyst Component
 White liquidPart A, Base Component
Mix Ratio10:1A:B

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Elkem (Bluestar Silicones) BLUESIL™ V-1062 Hi-Pro Green Silicone Rubber
Elkem (Bluestar Silicones) BLUESIL™ RTV 1556 B Fast Cure Silicone Rubber
Elkem (Bluestar Silicones) BLUESIL™ RTV 1556 B Silicone Rubber
Elkem (Bluestar Silicones) BLUESIL™ RTV 3165 A&B Silicone Rubber
Elkem (Bluestar Silicones) BLUESIL™ RTV 3611 A/B Silicone Rubber

PBLUST056 / 191032

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.