MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Schott N-ZK7 Glass
Categories: Ceramic; Glass

Material Notes:

Information Provided by SCHOTT North America, Inc.

Key Words: 508612.249
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.49 g/cc0.0900 lb/in³
 
Chemical PropertiesMetricEnglishComments
Acid Class, SR 2.02.0
Alkali Class, AR 1.21.2
Stain Resistance Class, FR 0.000.00
 
Mechanical PropertiesMetricEnglishComments
Knoop Microhardness 530530.1/20
Modulus of Elasticity 70.0 GPa10200 ksi
Poissons Ratio 0.2140.214
Shear Modulus 29.0 GPa4210 ksicalculated
 
Thermal PropertiesMetricEnglishComments
CTE, linear  4.50 µm/m-°C
@Temperature -30.0 - 70.0 °C
2.50 µin/in-°F
@Temperature -22.0 - 158 °F
 5.20 µm/m-°C
@Temperature 20.0 - 300 °C
2.89 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.770 J/g-°C0.184 BTU/lb-°F
Thermal Conductivity 1.042 W/m-K7.231 BTU-in/hr-ft²-°F
Transformation Temperature, Tg 539 °C1000 °F
Softening Point 721 °C1330 °FViscosity 107.6 dPa s
 
Optical PropertiesMetricEnglishComments
Refractive Index  1.50847
@Wavelength 587.6 nm
1.50847
@Wavelength 587.6 nm
nd
 1.51045
@Wavelength 546.1 nm
1.51045
@Wavelength 546.1 nm
ne
Abbe Number 60.9860.98ve
 61.1961.19vd
Optical Dispersion 0.008310.00831nf - nc
 0.008370.00837nf' - nc'
Transmission, Visible  98.2 %
@Thickness 10.0 mm,
Wavelength 380 nm
98.2 %
@Thickness 0.394 in,
Wavelength 380 nm
 99.1 %
@Thickness 10.0 mm,
Wavelength 405 nm
99.1 %
@Thickness 0.394 in,
Wavelength 405 nm
 99.5 %
@Thickness 10.0 mm,
Wavelength 460 nm
99.5 %
@Thickness 0.394 in,
Wavelength 460 nm
 99.8 %
@Thickness 10.0 mm,
Wavelength 580 nm
99.8 %
@Thickness 0.394 in,
Wavelength 580 nm
 99.8 %
@Thickness 10.0 mm,
Wavelength 700 nm
99.8 %
@Thickness 0.394 in,
Wavelength 700 nm
IR Transmittance  65.7 %
@Thickness 10.0 mm,
Wavelength 2500 nm
65.7 %
@Thickness 0.394 in,
Wavelength 2500 nm
 99 %
@Thickness 10.0 mm,
Wavelength 1530 nm
99 %
@Thickness 0.394 in,
Wavelength 1530 nm
UV Transmittance  3.2 %
@Thickness 10.0 mm,
Wavelength 290 nm
3.2 %
@Thickness 0.394 in,
Wavelength 290 nm
 22.1 %
@Thickness 10.0 mm,
Wavelength 300 nm
22.1 %
@Thickness 0.394 in,
Wavelength 300 nm
 85.2 %
@Thickness 10.0 mm,
Wavelength 334 nm
85.2 %
@Thickness 0.394 in,
Wavelength 334 nm
 97.6 %
@Thickness 10.0 mm,
Wavelength 370 nm
97.6 %
@Thickness 0.394 in,
Wavelength 370 nm
 
Descriptive Properties
B1
Climatic Resistance Test CR1
HG4
K (10-6mm2/N)3.63
Phosphate Resistance PR2.2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Corning Willow® Flexible Display Glass
Schott N-PK52A Glass
Ohara BSM51Y i-Line Optical Glass
Saint-Gobain Spectrosil® 2000 Optical Fused Quartz
Saint-Gobain Spectrosil® 2200 Optical Fused Quartz

CSGS013 / 93347

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.