MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ti-24.5Al-17Nb Titanium Aluminide
Categories: Metal; Intermetallic; Nonferrous Metal; Titanium Alloy

Material Notes: Titanium Aluminide Ti3Al based alloy. Ti-24.5Al-17Nb refers to the atomic percentage composition. The niobium addition of over > 15 atom%, and therefore formation of the O phase, improves toughness versus Ti3Al and lower Nb compositions. Intermetallic aluminides have good mechanical properties and stability to be used in high temperature environments. A thin protective Al2O3 coating forms to provide oxidative stability.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 940 MPa136000 psiWidmanstätten microstructure, primary alpha-2 grains
 1010 MPa146000 psiWidmanstätten microstructure
Tensile Strength, Yield 705 MPa102000 psiWidmanstätten microstructure, primary alpha-2 grains
 952 MPa138000 psiWidmanstätten microstructure
Elongation at Break 5.8 %5.8 %Widmanstätten microstructure
 10 %10 %Widmanstätten microstructure, primary alpha-2 grains
Creep Strength 380 MPa
@Temperature 650 °C,
Time 223000 sec
55100 psi
@Temperature 1200 °F,
Time 62.0 hour
Widmanstätten microstructure; Creep Rupture
Fracture Toughness 28.3 MPa-m½25.8 ksi-in½KIC; Widmanstätten microstructure
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 13.1 %13.1 %by weight
Niobium, Nb (Columbium, Cb) 31.3 %31.3 %by weight
Titanium, Ti 55.6 %55.6 %by weight

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ti-25Al-17Nb-1Mo Titanium Aluminide
Ti-24Al-14Nb Titanium Aluminide
Ti-25Al-10Nb-3V-1Mo Titanium Aluminide
Ti-24Al-11Nb Titanium Aluminide
Ti15Mo5Zr3Al ß titanium alloy

MIAL028 / 143025

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.