MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Zytel® 80G33HS1L NC010 PA66-IGF33
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: 33% Glass Reinforced, Toughened, Heat Stabilized, Polyamide 66

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.33 g/cc0.0480 lb/in³DAM; ISO 1183
Melt Density 1.12 g/cc
@Temperature 295 °C
0.0405 lb/in³
@Temperature 563 °F
Water Absorption 0.85 %
@Time 86400 sec
0.85 %
@Time 24.0 hour
Immersion; DAM; Sim. to ISO 62
 4.5 %
@Thickness 2.00 mm
4.5 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Moisture Absorption 1.50 %
@Thickness 2.00 mm
1.50 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Viscosity Number 144 cm³/g1.44 dl/gsulfuric acid 96%; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0030 cm/cm0.0030 in/inDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0070 cm/cm0.0070 in/inDAM; ISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7070DAM; ISO 2039-2
Hardness, Rockwell R 110110DAM; ISO 2039-2
Ball Indentation Hardness 220 MPa31900 psiH 961/30; DAM; ISO 2039-1
Tensile Strength at Break 108 MPa15700 psi50% RH; ISO 527-1/-2
 146 MPa21200 psiDAM; ISO 527-1/-2
Elongation at Break 3.7 %3.7 %DAM; ISO 527-1/-2
 7.0 %7.0 %50% RH; ISO 527-1/-2
Tensile Modulus 6.20 GPa899 ksi50% RH; ISO 527-1/-2
 8.90 GPa1290 ksiDAM; ISO 527-1/-2
Flexural Strength 205 MPa29700 psiDAM; ISO 178
Flexural Modulus 6.20 GPa899 ksi50% RH; ISO 178
 7.50 GPa1090 ksiDAM; ISO 178
Poissons Ratio 0.340.34DAM
 0.350.3550% RH
Izod Impact, Notched (ISO)  15.0 kJ/m²
@Temperature -40.0 °C
7.14 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 180/1A
 15.0 kJ/m²
@Temperature -40.0 °C
7.14 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 180/1A
 16.0 kJ/m²
@Temperature -30.0 °C
7.61 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 180/1A
 17.0 kJ/m²
@Temperature -30.0 °C
8.09 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1A
 21.0 kJ/m²
@Temperature 23.0 °C
9.99 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 26.0 kJ/m²
@Temperature 23.0 °C
12.4 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 180/1A
Izod Impact, Unnotched (ISO)  75.0 kJ/m²
@Temperature -30.0 °C
35.7 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 180/1U
 80.0 kJ/m²
@Temperature -30.0 °C
38.1 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1U
 80.0 kJ/m²
@Temperature 23.0 °C
38.1 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 180/1U
 80.0 kJ/m²
@Temperature 23.0 °C
38.1 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1U
Charpy Impact Unnotched  9.70 J/cm²
@Temperature 23.0 °C
46.2 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eU
 9.80 J/cm²
@Temperature 23.0 °C
46.6 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eU
 10.0 J/cm²
@Temperature -30.0 °C
47.6 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eU
 10.6 J/cm²
@Temperature -30.0 °C
50.4 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eU
Charpy Impact, Notched  1.40 J/cm²
@Temperature -40.0 °C
6.66 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 179/1eA
 1.70 J/cm²
@Temperature -30.0 °C
8.09 ft-lb/in²
@Temperature -22.0 °F
50% RH; ISO 179/1eA
 1.80 J/cm²
@Temperature -30.0 °C
8.57 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 1.80 J/cm²
@Temperature -40.0 °C
8.57 ft-lb/in²
@Temperature -40.0 °F
50% RH; ISO 179/1eA
 2.00 J/cm²
@Temperature 23.0 °C
9.52 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 2.80 J/cm²
@Temperature 23.0 °C
13.3 ft-lb/in²
@Temperature 73.4 °F
50% RH; ISO 179/1eA
Tensile Creep Modulus, 1 hour 5300 MPa769000 psi1h; 50% RH; ISO 899-1
Tensile Creep Modulus, 1000 hours 4300 MPa624000 psi1000h; 50% RH; ISO 899-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+11 ohm-cm1.00e+11 ohm-cm50% RH; IEC 62631-3-1
 >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmDAM; IEC 62631-3-1
Surface Resistance 1.00e+12 ohm1.00e+12 ohm50% RH; IEC 62631-3-2
Comparative Tracking Index 425 V425 V50% RH; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 15.0 µm/m-°C8.33 µin/in-°FDAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 120 µm/m-°C66.7 µin/in-°FDAM; ISO 11359-1/-2
Specific Heat Capacity 2.20 J/g-°C
@Temperature 295 °C
0.526 BTU/lb-°F
@Temperature 563 °F
Melt
Thermal Conductivity 0.220 W/m-K
@Temperature 295 °C
1.53 BTU-in/hr-ft²-°F
@Temperature 563 °F
Melt
Melting Point 262 °C504 °F10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 261 °C502 °FDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 246 °C475 °FDAM; ISO 75-1/-2
Vicat Softening Point 245 °C473 °F50°C/h, 50N; DAM; ISO 306
Glass Transition Temp, Tg 20.0 °C68.0 °F10°C/min; 50% RH; ISO 11357-1/-2
 75.0 °C167 °F10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94  HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
DAM; IEC 60695-11-10
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
DAM; IEC 60695-11-10
Flame Spread 23.0 mm/min
@Thickness 1.00 mm
0.906 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
 
Processing PropertiesMetricEnglishComments
Melt Temperature 295 °C563 °FOptimum, Injection
 285 - 305 °C545 - 581 °FRange, Injection
Mold Temperature 50.0 - 100 °C122 - 212 °FInjection
 80.0 °C176 °FOptimum, Injection
Ejection Temperature 210 °C410 °FInjection
Drying Temperature 80.0 °C176 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %<= 0.20 %Injection
Hold Pressure 50.0 - 100 MPa7250 - 14500 psiRange, Injection
 
Descriptive Properties
AdditivesRelease agent
Drying RecommendedyesInjection
Eff. thermal diffusivity (m²/s)9E-08
Emission of organic compounds (µgC/g)25VDA 277
FMVSS ClassSE/BISO 3795 (FMVSS 302)
Fogging (mg)0.8G-value (condensate); ISO 6452; DAM
ISO designationISO 16396-PA66-I,GF33,M1GHNR,S14-090
Max. screw tangential speed (m/s)0.2Injection
Odor Class3VDA 270
Part Marking Code>PA66-IGF33<ISO 11469
PolymerPA66-I-GF33
Processing Hold Pressure Time (s/mm)3Injection
Resin IdentificationPA66-IGF33ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Zytel® 80G33HS1L BK104 PA66-IGF33
Celanese Zytel® 70G33L BK031 PA66-GF33
Celanese Zytel® 80G33L NC010 PA66-IGF33
Celanese Zytel® 70G13HS1L BK031 PA66-GF13
Celanese Zytel® 70G13HS1L NC010 PA66-GF13

PDSX5381 / 198021

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.