MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LG Chemical LUPOY EF5001RFT PC/ABS
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced; Polycarbonate (PC)

Material Notes: Description: Injection Molding, PC/ABS, Halogen Free Flame Retardant, EU Eco-Label compliant

Application: Display housing

CAS: 103598-77-2, 9003-56-9 and 125997-21-9

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.19 g/cc1.19 g/ccASTM D792
Maximum Moisture Content 0.0400.040Injection Molding
Linear Mold Shrinkage, Flow 0.0040 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0040 - 0.0080 in/in
@Thickness 0.126 in
ASTM D955
Melt Flow 20 g/10 min
@Load 2.16 kg,
Temperature 250 °C
20 g/10 min
@Load 4.76 lb,
Temperature 482 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 56.9 MPa
@Thickness 3.20 mm
8250 psi
@Thickness 0.126 in
50mm/min; ASTM D638
Elongation at Break 30 %
@Thickness 3.20 mm
30 %
@Thickness 0.126 in
50mm/min; ASTM D638
Flexural Yield Strength 93.2 MPa
@Thickness 3.20 mm
13500 psi
@Thickness 0.126 in
10mm/min; ASTM D790
Flexural Modulus 2.45 GPa
@Thickness 3.20 mm
356 ksi
@Thickness 0.126 in
10mm/min; ASTM D790
Izod Impact, Notched >= 4.90 J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
>= 9.18 ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 94.0 °C
@Thickness 6.40 mm
201 °F
@Thickness 0.252 in
Unannealed; ASTM D648
UL RTI, Electrical 60.0 °C140 °F
UL RTI, Mechanical with Impact 60.0 °C140 °F
UL RTI, Mechanical without Impact 60.0 °C140 °F
Flammability, UL94  V-0
@Thickness >=1.60 mm
V-0
@Thickness >=0.0630 in
 V-0
@Thickness >=3.20 mm
V-0
@Thickness >=0.126 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 230 - 250 °C446 - 482 °FInjection Molding
Middle Barrel Temperature 230 - 250 °C446 - 482 °FInjection Molding
Front Barrel Temperature 230 - 250 °C446 - 482 °FInjection Molding
Nozzle Temperature 230 - 250 °C446 - 482 °FInjection Molding
Melt Temperature 240 - 260 °C464 - 500 °FInjection Molding
Mold Temperature 60.0 - 80.0 °C140 - 176 °FInjection Molding
Drying Temperature 75.0 - 85.0 °C167 - 185 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
Back Pressure 0.981 - 3.92 MPa142 - 569 psiInjection Molding
Screw Speed 40 - 70 rpm40 - 70 rpmInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LG Chemical LUPOY ER5001RF PC/ABS
LG Chemical LUPOY GN5001RF PC/ABS, Halogen Free Flame Retardant
LG Chemical LUPOY GN5001RFD PC/ABS, High Impact
LG Chemical LUPOY GN1008RF PC, Halogen Free, Flame Retardant, High impact strength
LG Chemical LUPOY GN1002FS PC, Halogen Free, Flame Retardant, High Impact

PLAY577 / 148587

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.