Physical Properties | Metric | English | Comments |
---|
Density | 8.97 g/cc | 0.324 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Ultimate | 860 MPa | 125000 psi |
| 55.0 MPa @Temperature 1204 °C | 7980 psi @Temperature 2199 °F |
| 79.0 MPa @Temperature 1149 °C | 11500 psi @Temperature 2100 °F |
| 120 MPa @Temperature 1093 °C | 17400 psi @Temperature 1999 °F |
| 225 MPa @Temperature 982 °C | 32600 psi @Temperature 1800 °F |
| 400 MPa @Temperature 871 °C | 58000 psi @Temperature 1600 °F |
| 585 MPa @Temperature 760 °C | 84800 psi @Temperature 1400 °F |
| 670 MPa @Temperature 649 °C | 97200 psi @Temperature 1200 °F |
| 710 MPa @Temperature 538 °C | 103000 psi @Temperature 1000 °F |
Tensile Strength, Yield | 390 MPa @Strain 0.2 % | 56600 psi @Strain 0.2 % |
| 26.0 MPa @Strain 0.2 %, Temperature 1204 °C | 3770 psi @Strain 0.2 %, Temperature 2199 °F |
| 39.0 MPa @Strain 0.2 %, Temperature 1149 °C | 5660 psi @Strain 0.2 %, Temperature 2100 °F |
| 57.0 MPa @Strain 0.2 %, Temperature 1093 °C | 8270 psi @Strain 0.2 %, Temperature 1999 °F |
| 120 MPa @Strain 0.2 %, Temperature 982 °C | 17400 psi @Strain 0.2 %, Temperature 1800 °F |
| 225 MPa @Strain 0.2 %, Temperature 871 °C | 32600 psi @Strain 0.2 %, Temperature 1600 °F |
| 270 MPa @Strain 0.2 %, Temperature 649 °C | 39200 psi @Strain 0.2 %, Temperature 1200 °F |
| 275 MPa @Strain 0.2 %, Temperature 538 °C | 39900 psi @Strain 0.2 %, Temperature 1000 °F |
| 285 MPa @Strain 0.2 %, Temperature 760 °C | 41300 psi @Strain 0.2 %, Temperature 1400 °F |
Elongation at Break | 47.7 % | 47.7 % |
| 31.2 % @Temperature 1204 °C | 31.2 % @Temperature 2199 °F |
| 39.5 % @Temperature 1149 °C | 39.5 % @Temperature 2100 °F |
| 46.1 % @Temperature 760 °C | 46.1 % @Temperature 1400 °F |
| 49.6 % @Temperature 1093 °C | 49.6 % @Temperature 1999 °F |
| 55 % @Temperature 649 °C | 55 % @Temperature 1200 °F |
| 55.7 % @Temperature 538 °C | 55.7 % @Temperature 1000 °F |
| 58.9 % @Temperature 871 °C | 58.9 % @Temperature 1600 °F |
| 70.5 % @Temperature 982 °C | 70.5 % @Temperature 1800 °F |
Modulus of Elasticity | 211 GPa | 30600 ksi |
| 150 GPa @Temperature 1000 °C | 21800 ksi @Temperature 1830 °F |
| 157 GPa @Temperature 900 °C | 22800 ksi @Temperature 1650 °F |
| 164 GPa @Temperature 800 °C | 23800 ksi @Temperature 1470 °F |
| 171 GPa @Temperature 700 °C | 24800 ksi @Temperature 1290 °F |
| 177 GPa @Temperature 600 °C | 25700 ksi @Temperature 1110 °F |
| 184 GPa @Temperature 500 °C | 26700 ksi @Temperature 932 °F |
| 190 GPa @Temperature 400 °C | 27600 ksi @Temperature 752 °F |
| 196 GPa @Temperature 300 °C | 28400 ksi @Temperature 572 °F |
| 202 GPa @Temperature 200 °C | 29300 ksi @Temperature 392 °F |
| 207 GPa @Temperature 100 °C | 30000 ksi @Temperature 212 °F |
Charpy Impact | 73.0 J | 53.8 ft-lb |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000125 ohm-cm | 0.000125 ohm-cm |
| 0.000125 ohm-cm @Temperature 1000 °C | 0.000125 ohm-cm @Temperature 1830 °F |
| 0.0001258 ohm-cm @Temperature 100 °C | 0.0001258 ohm-cm @Temperature 212 °F |
| 0.0001265 ohm-cm @Temperature 200 °C | 0.0001265 ohm-cm @Temperature 392 °F |
| 0.0001271 ohm-cm @Temperature 900 °C | 0.0001271 ohm-cm @Temperature 1650 °F |
| 0.0001273 ohm-cm @Temperature 300 °C | 0.0001273 ohm-cm @Temperature 572 °F |
| 0.0001284 ohm-cm @Temperature 400 °C | 0.0001284 ohm-cm @Temperature 752 °F |
| 0.0001291 ohm-cm @Temperature 800 °C | 0.0001291 ohm-cm @Temperature 1470 °F |
| 0.0001302 ohm-cm @Temperature 500 °C | 0.0001302 ohm-cm @Temperature 932 °F |
| 0.0001307 ohm-cm @Temperature 700 °C | 0.0001307 ohm-cm @Temperature 1290 °F |
| 0.0001312 ohm-cm @Temperature 600 °C | 0.0001312 ohm-cm @Temperature 1110 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.7 µm/m-°C @Temperature 25.0 - 100 °C | 7.06 µin/in-°F @Temperature 77.0 - 212 °F |
| 13.0 µm/m-°C @Temperature 25.0 - 200 °C | 7.22 µin/in-°F @Temperature 77.0 - 392 °F |
| 13.3 µm/m-°C @Temperature 25.0 - 300 °C | 7.39 µin/in-°F @Temperature 77.0 - 572 °F |
| 13.7 µm/m-°C @Temperature 25.0 - 400 °C | 7.61 µin/in-°F @Temperature 77.0 - 752 °F |
| 14.0 µm/m-°C @Temperature 25.0 - 500 °C | 7.78 µin/in-°F @Temperature 77.0 - 932 °F |
| 14.4 µm/m-°C @Temperature 25.0 - 600 °C | 8.00 µin/in-°F @Temperature 77.0 - 1110 °F |
| 14.8 µm/m-°C @Temperature 25.0 - 700 °C | 8.22 µin/in-°F @Temperature 77.0 - 1290 °F |
| 15.2 µm/m-°C @Temperature 25.0 - 800 °C | 8.44 µin/in-°F @Temperature 77.0 - 1470 °F |
| 15.7 µm/m-°C @Temperature 25.0 - 900 °C | 8.72 µin/in-°F @Temperature 77.0 - 1650 °F |
| 16.1 µm/m-°C @Temperature 25.0 - 1000 °C | 8.94 µin/in-°F @Temperature 77.0 - 1830 °F |
Specific Heat Capacity | 0.397 J/g-°C | 0.0949 BTU/lb-°F |
| 0.419 J/g-°C @Temperature 100 °C | 0.100 BTU/lb-°F @Temperature 212 °F |
| 0.435 J/g-°C @Temperature 200 °C | 0.104 BTU/lb-°F @Temperature 392 °F |
| 0.448 J/g-°C @Temperature 300 °C | 0.107 BTU/lb-°F @Temperature 572 °F |
| 0.465 J/g-°C @Temperature 400 °C | 0.111 BTU/lb-°F @Temperature 752 °F |
| 0.473 J/g-°C @Temperature 500 °C | 0.113 BTU/lb-°F @Temperature 932 °F |
| 0.486 J/g-°C @Temperature 600 °C | 0.116 BTU/lb-°F @Temperature 1110 °F |
| 0.574 J/g-°C @Temperature 700 °C | 0.137 BTU/lb-°F @Temperature 1290 °F |
| 0.595 J/g-°C @Temperature 800 °C | 0.142 BTU/lb-°F @Temperature 1470 °F |
| 0.609 J/g-°C @Temperature 900 °C | 0.146 BTU/lb-°F @Temperature 1650 °F |
| 0.617 J/g-°C @Temperature 1000 °C | 0.147 BTU/lb-°F @Temperature 1830 °F |
Thermal Conductivity | 8.90 W/m-K | 61.8 BTU-in/hr-ft²-°F |
| 10.4 W/m-K @Temperature 100 °C | 72.2 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 12.4 W/m-K @Temperature 200 °C | 86.1 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 14.4 W/m-K @Temperature 300 °C | 99.9 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 16.4 W/m-K @Temperature 400 °C | 114 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 18.4 W/m-K @Temperature 500 °C | 128 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 20.4 W/m-K @Temperature 600 °C | 142 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 22.4 W/m-K @Temperature 700 °C | 155 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 24.4 W/m-K @Temperature 800 °C | 169 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 26.4 W/m-K @Temperature 900 °C | 183 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 28.4 W/m-K @Temperature 1000 °C | 197 BTU-in/hr-ft²-°F @Temperature 1830 °F |
Melting Point | 1301 - 1371 °C | 2374 - 2500 °F |
Solidus | 1301 °C | 2374 °F |
Liquidus | 1371 °C | 2500 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 0.30 % | 0.30 % |
Boron, B | <= 0.015 % | <= 0.015 % |
Carbon, C | 0.10 % | 0.10 % |
Chromium, Cr | 22 % | 22 % |
Cobalt, Co | <= 5.0 % | <= 5.0 % |
Iron, Fe | <= 3.0 % | <= 3.0 % |
Lanthanum, La | 0.020 % | 0.020 % |
Manganese, Mn | 0.50 % | 0.50 % |
Molybdenum, Mo | 2.0 % | 2.0 % |
Nickel, Ni | 57 % | 57 % |
Silicon, Si | 0.40 % | 0.40 % |
Tungsten, W | 14 % | 14 % |