MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

CHT Group AS1802 (1084G) SILCOTHERM 1 Part RTV silicone adhesive
Categories: Polymer; Adhesive

Material Notes: AS1802 is a non-corrosive, 1-part, room temperature vulcanising (RTV) silicone rubber. It is one of a new family of products called acetone cure sealants that are solvent free. It exhibits excellent primerless adhesion to many substrates. The product is cured rapidly in contact with atmospheric moisture to a tough rubber. It does not corrode copper or its alloys and exhibits excellent primerless adhesion when fully cured.

Key Features:

  • Excellent thermal conductivity
  • Non-corrosive
  • Fast skinning
  • Low linear shrinkage
  • Will meet the requirements of UL 94 V-0

Formerly Amber Chemical Co (ACC Silicones), aquired by CHT in 2017

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.11 g/cc2.11 g/ccafter 7 days cure at 23+/-2°C and 65% relative humidity; BS 903 Part A1
Linear Mold Shrinkage 0.0050 cm/cm0.0050 in/inafter 7 days cure at 23+/-2°C and 65% relative humidity
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6767after 7 days cure at 23+/-2°C and 65% relative humidity; ASTM D 2240-95
Tensile Strength 3.90 MPa566 psiafter 7 days cure at 23+/-2°C and 65% relative humidity; BS903 Part A2
Elongation at Break 103 %103 %after 7 days cure at 23+/-2°C and 65% relative humidity; BS903 Part A2
Adhesive Bond Strength 0.292 MPa42.4 psiOverlap Shear Strength, Stainless Steel 304; ASTM D1002
 0.353 MPa51.2 psiOverlap Shear Strength, Copper; ASTM D1002
 0.701 MPa102 psiOverlap Shear Strength, Aluminum; ASTM D1002
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmASTM D257
Dielectric Constant 4.9
@Frequency 1e+6 Hz
4.9
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 20.0 kV/mm508 kV/inASTM D149
Dissipation Factor 0.00090
@Frequency 1e+6 Hz
0.00090
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 164 µm/m-°C91.1 µin/in-°Fafter 7 days cure at 23+/-2°C and 65% relative humidity
Thermal Conductivity 2.30 W/m-K16.0 BTU-in/hr-ft²-°Fafter 7 days cure at 23+/-2°C and 65% relative humidity
Maximum Service Temperature, Air 220 °C428 °Fafter 7 days cure at 23+/-2°C and 65% relative humidity; AFS 1540B
Minimum Service Temperature, Air -50.0 °C-58.0 °Fafter 7 days cure at 23+/-2°C and 65% relative humidity
 
Processing PropertiesMetricEnglishComments
Cure Time 10100 min
@Temperature 21.0 - 25.0 °C
168 hour
@Temperature 69.8 - 77.0 °F
65% relative humidity
 <= 480 min
@Thickness 3.00 mm
<= 8.00 hour
@Thickness 0.118 in
Cure Through, 23+/-2°C and 65% relative humidity
Tack-Free Time 4.00 min0.0667 hour23+/-2°C and 65% relative humidity
 
Descriptive Properties
AppearanceGrey Paste
ColorGrey

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aptek 2712-A/B Very low stress silicone adhesive
Elkem (Bluestar Silicones) BLUESIL™ RTV 3611 A/B Silicone Rubber
Humiseal 1C49 Silicone Conformal Coating
Humiseal 1C51 Silicone Conformal Coating
Humiseal 1C55 Silicone Conformal Coating

PACC2004 / 199392

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.