MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lehvoss LUVOCOM® 1105/BK0873 PEEK unreinforced  (discontinued **)
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Unreinforced

Material Notes: Properties/attributes include: Highly chemically-resistant parts, non flammable. Especially suitable for medical parts, superheated steam sterilizable, hydrolysis resistance Inherent flame resistance.

Automotive industry, textile machinery, medical- and precision engineering, aircraft industry.

Processing: During processing, the moisture content should not exceed 0.05%. To avoid internal stresses, a medium to high injection rate should be used. An increase in tool temperature may be helpful. Post-crystallization may lead to warpage at elevated operating temperatures. This can be counteracted by suitable heat treatment. The processing notes provided merely represent a recommendation for general use. Due to the large variety of machines, geometries and volumes of parts, etc., it may be necessary to employ different settings according to the specific application. High-temperature polymers place increased demands on the tool steels employed.

Information provided by Lehmann & Voss & Co.KG

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.32 g/cc1.32 g/ccISO 1183
Moisture Absorption 0.500 %
@Temperature 23.0 °C,
Time 86400 sec
0.500 %
@Temperature 73.4 °F,
Time 24.0 hour
Linear Mold Shrinkage 0.010 - 0.016 cm/cm0.010 - 0.016 in/inDIN 16901
Melt Flow 32 g/10 min
@Load 10.0 kg,
Temperature 380 °C
32 g/10 min
@Load 22.0 lb,
Temperature 716 °F
(MVR); ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 100 MPa14500 psiISO 527-2
Elongation at Break 5.0 %5.0 %ISO 527-2
Modulus of Elasticity 4.00 GPa580 ksiISO 527-2
Flexural Strength 145 MPa21000 psiISO 178
Flexural Modulus 3.50 GPa508 ksiISO 178
Flexural Strain at Break 6.0 %6.0 %Flexural Elongation @ Fmax; ISO 178
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity >= 1.00e+12 ohm-cm>= 1.00e+12 ohm-cmIEC 60167
 
Thermal PropertiesMetricEnglishComments
CTE, linear 47.0 µm/m-°C26.1 µin/in-°FDIN 53752
Thermal Conductivity 0.250 W/m-K1.74 BTU-in/hr-ft²-°FDIN 52612
Maximum Service Temperature, Air 250 °C482 °FContinuous; UL 746B
 260 °C500 °FShort Term
Deflection Temperature at 1.8 MPa (264 psi) 152 °C306 °FISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 360 - 380 °C680 - 716 °F
Zone 1 360 - 370 °C680 - 698 °F
Zone 2 380 - 390 °C716 - 734 °F
Zone 3 390 - 400 °C734 - 752 °F
Melt Temperature 390 °C734 °F
Mold Temperature 170 - 190 °C338 - 374 °FSuggested Range
Drying Temperature  120 °C
@Time 21600 - 28800 sec
248 °F
@Time 6.00 - 8.00 hour
Dehumidifying dryer
 150 °C
@Time 10800 - 21600 sec
302 °F
@Time 3.00 - 6.00 hour
Dehumidifying dryer
Moisture Content <= 0.050 %<= 0.050 %
 
Descriptive Properties
Colorblack

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyetheretherketone, Unreinforced
Mitsubishi Chemical Advanced Materials Ketron™ 1000 PEEK, Extruded Unfilled Polyetherether Ketone
Evonik VESTAKEEP® 1000P PEEK
Evonik VESTAKEEP® 4000P PEEK
Akro-Plastic Akrotek® PEEK natural (5184) PEEK, Dry

PLUU8818 / 193777

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.