MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil Exceed™ PP9122 Polypropylene Homopolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: Product Description: A random copolymer resin designed for extrusion blow molding applications and thermoforming of medical and other specialty devices and packaging. It has excellent organoleptics and very low ash metal content.

Availability: North America

Features:

  • Autoclave Sterilizable
  • Clean/High Purity
  • Ethylene Oxide Sterilizable
  • Low Extractables
  • Low to No Odor
  • Steam Sterilizable
Uses:
  • Caps
  • Closures
  • Labware
  • Medical Packaging
  • Medical/Healthcare Applications
  • Packaging
Processing Method: Blow Molding, Extrusion, Extrusion Blow Molding, Injection Blow Molding, Profile Extrusion, Sheet Extrusion and Thermoforming

Information provided by ExxonMobil

Key Words: ExxonMobil ™ PP9122
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ExxonMobil Method
Melt Flow 2.1 g/10 min
@Load 2.16 kg,
Temperature 230 °C
2.1 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 28.5 MPa4140 psi2.0 in/min; ASTM D638
Elongation at Yield 13 %13 %2.0 in/min; ASTM D638
Flexural Modulus, 1% Secant 972 MPa141000 psi0.05 in/min; ASTM D790A
 1140 MPa166000 psi0.5 in/min; ASTM D790B
Izod Impact, Notched 0.694 J/cm1.30 ft-lb/inASTM D256A
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 81.7 °C179 °FASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil PP1013H1 Polypropylene Homopolymer
ExxonMobil PP1074KNE1 Polypropylene Homopolymer
ExxonMobil PP6262 Polypropylene Homopolymer
ExxonMobil PP1014H1 Polypropylene Homopolymer
ExxonMobil ACHIEVE 1605 Exxpol Metallocene Grade for Injection Molding Applications

PEX99415 / 175651

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.