Envalior Durethan® B 30 S 000000 Nylon 6 (PA6), Dry
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, Unreinforced
Material Notes:
PA 6, injection molding-grade, non-reinforced, easy-flow, easy-release, rapid solidification
Former Lanxess product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Bulk Density
0.700
g/cc
0.0253
lb/in³
ISO 60
Density
1.14
g/cc
0.0412
lb/in³
ISO 1183
Moisture Absorption at Equilibrium
3.0 %
3.0 %
50% RH; ISO 62
Water Absorption at Saturation
10 %
10 %
ISO 62
Linear Mold Shrinkage, Flow
0.0102
cm/cm
0.0102
in/in
150x105x3; 260 °C / MT 80 °C; 500 bar; ISO 294-4
Linear Mold Shrinkage, Transverse
0.0116
cm/cm
0.0116
in/in
150x105x3; 260 °C / MT 80 °C; 500 bar; ISO 294-4
Mechanical Properties
Metric
English
Comments
Puncture Resistance
5141
N
@Temperature 23.0 °C
1156
lb (f)
@Temperature 73.4 °F
ISO 6603-2
6543
N
@Temperature -30.0 °C
1471
lb (f)
@Temperature -22.0 °F
ISO 6603-2
Ball Indentation Hardness
140
MPa
20300
psi
ISO 2093-1
Tensile Strength, Yield
80.0
MPa
11600
psi
50 mm/min; ISO 527-1,-2
Elongation at Break
20 %
20 %
50 mm/min, Nominal; ISO 527-1,-2
Elongation at Yield
4.0 %
4.0 %
50 mm/min; ISO 527-1,-2
Tensile Modulus
3.20
GPa
464
ksi
1 mm/min; ISO 527-1,-2
Flexural Strength
110
MPa
16000
psi
2 mm/min; ISO 178-A
Flexural Yield Strength
95.0
MPa
@Strain 3.5 %
13800
psi
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus
2.90
GPa
421
ksi
2 mm/min; ISO 178-A
Flexural Strain at Break
6.0 %
6.0 %
2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)
<=
10.0
kJ/m²
@Temperature 23.0 °C
<=
4.76
ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
Izod Impact, Unnotched (ISO)
NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 180-1U
NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 180-1U
Charpy Impact Unnotched
NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179-1eU
NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179-1eU
Charpy Impact, Notched
<=
1.00
J/cm²
@Temperature 23.0 °C
<=
4.76
ft-lb/in²
@Temperature 73.4 °F
ISO 179 1eA
<=
1.00
J/cm²
@Temperature -30.0 °C
<=
4.76
ft-lb/in²
@Temperature -22.0 °F
ISO 179 1eA
Puncture Energy
10.0
J
@Temperature -30.0 °C
7.38
ft-lb
@Temperature -22.0 °F
ISO 6603-2
12.0
J
@Temperature 23.0 °C
8.85
ft-lb
@Temperature 73.4 °F
ISO 6603-2
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+13
ohm-cm
1.00e+13
ohm-cm
IEC 60093
Surface Resistance
1.00e+14
ohm
1.00e+14
ohm
IEC 60093
Dielectric Constant
3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
IEC 60250
4.0
@Frequency 100 Hz
4.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength
30.0
kV/mm
@Thickness 1.00 mm
762
kV/in
@Thickness 0.0394 in
IEC 60243-1
Dissipation Factor
0.017
@Frequency 100 Hz
0.017
@Frequency 100 Hz
IEC 60250
0.020
@Frequency 1e+6 Hz
0.020
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index
600
V
600
V
Solution A; IEC 60112
600
V
600
V
Solution B; IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
100
µm/m-°C
@Temperature 23.0 - 55.0 °C
55.6
µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
CTE, linear, Transverse to Flow
110
µm/m-°C
@Temperature 23.0 - 55.0 °C
61.1
µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Melting Point
222
°C
432
°F
10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi)
160
°C
320
°F
ISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi)
55.0
°C
131
°F
ISO 75-1,-2
Deflection Temperature at 8.0 MPa
45.0
°C
113
°F
ISO 75-1,-2
Vicat Softening Point
200
°C
@Load 5.10 kg
392
°F
@Load 11.2 lb
120°C/h; ISO 306
200
°C
@Load 5.10 kg
392
°F
@Load 11.2 lb
50°C/h; ISO 306
Oxygen Index
26 %
26 %
Method A; ISO 4589-2
Glow Wire Flammability Index
750
°C
@Thickness 2.00 mm
1380
°F
@Thickness 0.0787 in
IEC 60695-2-12
Shrinkage, MD
0.32 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.32 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Flow Direction Post-Molding, 150x105x3; ISO 294-4
Shrinkage, TD
0.40 %
@Treatment Temp. 120 °C,
Time 14400 sec
0.40 %
@Treatment Temp. 248 °F,
Time 4.00 hour
Post-Molding, 150x105x3; ISO 294-4
Processing Properties
Metric
English
Comments
Melt Temperature
270
°C
518
°F
injection molding; ISO 294
260
-
280
°C
500
-
536
°F
Mold Temperature
80.0
°C
176
°F
injection molding; ISO 294
80.0
-
100
°C
176
-
212
°F
Drying Temperature
80.0
°C
176
°F
Dry Time
2.00
-
6.00
hour
2.00
-
6.00
hour
Moisture Content
0.030 - 0.12 %
0.030 - 0.12 %
Karl Fischer
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Envalior Durethan® B 30 S 000000 Nylon 6 (PA6), Conditioned
BASF Ultramid® 8267G HS BK-106 15/25% Glass/Mineral Filled PA6 (Dry)
Envalior Akulon® K222-D PA6, Dry, Low Viscosity
Envalior Akulon® K224-G6U (Dry) 33% Glass Reinforced Nylon 6 (North America)
Envalior Akulon® K222-D PA6, Conditioned, Low Viscosity
PLANW9256 / 208057
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.