MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

17-7 PH Stainless Steel, cold rolled condition C, plate, sheet, and strip
Categories: Metal; Ferrous Metal; Stainless Steel; Precipitation Hardening Stainless; T S10000 Series Stainless Steel

Material Notes: Processing: Condition C - heated to austenitic range, 1040°C (1900°F), and water quenched. Severely cold worked (60-70%). The cold working induces a martensite transformation in the austenite.

Applications: high strength high temperature applications, chemical processing equipment, heat exchangers, power boilers, superheater tubes

Corrosion Resistance: 17-7 PH is suitable for use in fresh water, industrial and marine atmospheres, and mild chemical and oxidizing environments. 17-7 PH should not be used in salt water or reducing environments.

Key Words: UNS S17700, double treatment alloy, cold rolled condition C, 17-7PH, 17-7 PH, 17/7PH, 17/7 PH, Precipitation Hardening
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 4141
Tensile Strength, Ultimate 1380 MPa200000 psi
Tensile Strength, Yield 1210 MPa175000 psi
Elongation at Break 1.0 %1.0 %
Modulus of Elasticity 204 GPa29600 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000830 ohm-cm0.0000830 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.0 µm/m-°C
@Temperature 0.000 - 100 °C
6.11 µin/in-°F
@Temperature 32.0 - 212 °F
 11.6 µm/m-°C
@Temperature 0.000 - 315 °C
6.44 µin/in-°F
@Temperature 32.0 - 599 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
0.110 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity  16.4 W/m-K
@Temperature 100 °C
114 BTU-in/hr-ft²-°F
@Temperature 212 °F
 21.8 W/m-K
@Temperature 500 °C
151 BTU-in/hr-ft²-°F
@Temperature 932 °F
Melting Point 1400 - 1450 °C2550 - 2640 °F
Solidus 1400 °C2550 °F
Liquidus 1450 °C2640 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.75 - 1.5 %0.75 - 1.5 %
Carbon, C <= 0.090 %<= 0.090 %
Chromium, Cr 16 - 18 %16 - 18 %
Iron, Fe 70.6 - 76.8 %70.6 - 76.8 %as balance
Manganese, Mn <= 1.0 %<= 1.0 %
Nickel, Ni 6.5 - 7.75 %6.5 - 7.75 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.040 %<= 0.040 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
17-7 PH Stainless Steel, CH900, plate, sheet, and strip
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 900
17-7 PH Stainless Steel, RH950, plate, sheet, and strip
17-7 PH Stainless Steel, RH950, bar and forgings
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition A

MQM177G / 13562

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.