MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Hifax TRC 779X BLACK Thermoplastic Olefinic Elastomer, mineral Filled
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Olefinic Elastomer (TPO)

Material Notes: Hifax polypropylene resins based on the Catalloy process are used in applications such as building and construction (e.g., single-ply roofing), industrial applications (e.g., wire and cable), and automotive industries. Hifax priovides good processability, excellent impact resistance, a broad range of stiffness from very soft to rigid products, high temperature resistance and low linear coefficient of thermal expansion.

Hifax TRC 779X BLACK high melt flow, 1,700 MPa flexural modulus, paintable, mineral-filled thermoplastic elastomeric olefin (TEO) resin has an excellent balance of properties and processability. It is typically used for multiple automotive exterior applications. Applications: Automotive Parts, Bumpers, Exterior Automotive Applications.

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.00 g/cc0.0361 lb/in³Method A; ISO 1183
Melt Flow 25 g/10 min
@Load 2.16 kg,
Temperature 230 °C
25 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D 1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 18.0 MPa2610 psiISO 527-1,-2
Elongation at Yield 5.0 %5.0 %ISO 527-1,-2
Flexural Modulus 1.70 GPa247 ksiISO 178
Izod Impact, Notched (ISO)  6.50 kJ/m²
@Temperature -40.0 °C
3.09 ft-lb/in²
@Temperature -40.0 °F
ISO 180
 46.0 kJ/m²
@Temperature 23.0 °C
21.9 ft-lb/in²
@Temperature 73.4 °F
ISO 180
Impact Test 23.0 J
@Temperature -40.0 °C
17.0 ft-lb
@Temperature -40.0 °F
Multi-axial Impact Strength, 2.2m/s,3.2mm plaque, ductile failure mode; ASTM D 3763
 
Descriptive Properties
Processing MethodInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Hifax TRC 779X BLK Thermoplastic Olefinic Elastomer, mineral Filled
LyondellBasell Hifax TRC 779X 1 BLACK Polypropylene with 20% Talc
LyondellBasell Hifax TRC 779X SHS BLACK Thermoplastic Olefinic Elastomer, mineral Filled
LyondellBasell Hifax TRC 779X LD C1 BLACK Thermoplastic Olefinic Elastomer, mineral Filled
LyondellBasell Hifax TYC 773X BLK Thermoplastic Olefinic Elastomer, mineral Filled

PEQT7402 / 219039

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.