MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

BASF Ultradur® B 4330 G6 HR 30% Glass Filled PBT
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled

Material Notes: Description: Is a PBT-I, injection-molding grade with 30% glass fibers, for rigid, tough and dimensionally stable technical parts with increased requirements on hydrolysis resistance and toughness, e.g. automotive connectors and housings for electronic units under the hood.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.49 g/cc0.0538 lb/in³ISO 1183
Moisture Absorption at Equilibrium 0.20 %0.20 %23°C; 50% RH
Water Absorption at Saturation 0.40 %0.40 %DIN 53495/1L
Viscosity Test 108 cm³/g1.08 dl/gViscosity number; ISO 1628
Linear Mold Shrinkage, Flow 0.0050 cm/cm0.0050 in/in60x60x2 mm; ISO 294
Linear Mold Shrinkage, Transverse 0.011 cm/cm0.011 in/in60x60x2 mm; ISO 294
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 120 MPa17400 psi50 mm/min; ISO 527-2
Elongation at Break 3.4 %3.4 %50mm/min; ISO 527-2
Modulus of Elasticity 8.50 GPa1230 ksiISO 527-2
Charpy Impact Unnotched  6.00 J/cm²
@Temperature -30.0 °C
28.6 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 7.40 J/cm²
@Temperature 23.0 °C
35.2 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 1.40 J/cm²6.66 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 - 225 °C428 - 437 °FDSC; ISO 11357-3
Maximum Service Temperature, Air 210 °C410 °F
Deflection Temperature at 0.46 MPa (66 psi) 220 °C428 °FISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 205 °C401 °FISO 75-2
Decomposition Temperature >= 290 °C>= 554 °F
Flammability, UL94  HB
@Thickness 0.800 mm
HB
@Thickness 0.0315 in
 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
Ignition Temperature 350 °C662 °FASTM D1929
 
Processing PropertiesMetricEnglishComments
Processing Temperature 80.0 °C176 °FHopper Throat
Zone 1 250 °C482 °FFeeding zone
Zone 2 255 °C491 °FCompression
Zone 3 260 °C500 °FMetering-zone
Zone 4 260 °C500 °FNozzle
Melt Temperature 260 °C500 °FOptimal
 250 - 280 °C482 - 536 °FInjection-molding
Mold Temperature 60.0 - 100 °C140 - 212 °FInjection molding
 80.0 °C176 °FOptimal
Drying Temperature 80.0 - 120 °C176 - 248 °F
Dry Time 4 hour4 hour
 
Descriptive Properties
ColorNatural and Black
Commercial StatusEurope
Peripheral Screw Speed<0.25 m/s
Primary Processing TechniqueInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultradur® B 4300 G6 30% Glass Filled PBT
BASF Ultradur® B 4300 G6 HR 30% Glass Filled PBT
BASF Ultradur® B 4300 G4 High Speed Unc. 20% Glass Filled PBT
BASF Ultradur® B 4300 G4 FC 20% Glass Filled PBT
BASF Ultradur® B 4300 M5 25% Mineral Filled PBT

PBASG0116 / 131750

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.