MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Lupolen 3621 M RM Linear Low Density Polyethylene (LLDPE), Rotational Molding Grade
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Rotational Molding Grade

Material Notes: Lupolen 3621 M RM is a new generation hexene linear low density polyethylene for rotational molding. Typical customer applications include agricultural and chemical storage containers and technical parts. This product exhibits excellent ESCR and high impact strength at low temperatures. Lupolen 3621 M RM is a UV-stabilized and pelletized polymer. Tests have shown that this material is resists the harmful effect of biodiesel fuel. It is not intended for use in medical and pharmaceutical applications. Applications: Crates, Heavy Duty Packaging, Industrial, Industrial Packaging, Intermediate Bulk Containers, Tanks, Industrial

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.9355 g/cc0.03380 lb/in³ISO 1183-1
Environmental Stress Crack Resistance >= 1000 hour>= 1000 hourcond. B, 10% Arkopal N100; ASTM D1693
Melt Flow 7.5 g/10 min
@Load 2.16 kg,
Temperature 190 °C
7.5 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133-1
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 17.0 MPa2470 psiISO 527-1,-2
Elongation at Break >= 450 %>= 450 %ISO 527-1,-2
Elongation at Yield 10 %10 %ISO 527-1,-2
Tensile Modulus 0.700 GPa102 ksiISO 527-1,-2
Tensile Impact Strength 104 kJ/m²
@Temperature -30.0 °C
49.5 ft-lb/in²
@Temperature -22.0 °F
notched, type 1, method A; ISO 8256
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 113 °C235 °FA50N; ISO 306
 
Descriptive Properties
FNCT (hrs)15ISO 16770, 6.0 MPa, 2% Arkopal N100, 50°C
Peak Internal Air Temperature180-210°C, should not exceed 325°C
Processing MethodRotomolding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Bamberger Polymers Bapolene® 3042U Polyethylene, Rotational Molding Grade
Braskem ML4400N LLDPE Rotomolding Polyethylene
Braskem ML3601U LLDPE Rotomolding Polyethylene
Overview of materials for Linear Low Density Polyethylene (LLDPE), Rotational Molding Grade
Versalis Clearflex® RP 50 U Linear Medium Density Polyethylene

PEQT8553 / 220188

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.