MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

EDRO #3 Prehardened Mold Quality P20 Alloy Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Chrome-moly Steel

Material Notes: EDRO #3™ is a vacuum-degassed, ladle refined, Cr-Ni-Mo- alloyed steel which is supplied in the hardened and tempered condition.
EDRO #3™ is manufactured to consistently high quality standards with a very low sulfur content, giving a steel with the following characteristics: excellent polishing and photo-etching properties, good machinability, high purity and good homogeneity, and uniform hardness in all dimensions.
Applications: injection molds for thermo-plastics, extrusion dies for thermo-plastics, blow molds, forming tools, press-brake dies, structural components, shafts

Information provided by EDRO

Key Words: AISI P20 improved, W.-Nr. 1.2710
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density  7.67 g/cc
@Temperature 399 °C
0.277 lb/in³
@Temperature 750 °F
Hardened and tempered to 310 HB
 7.75 g/cc
@Temperature 199 °C
0.280 lb/in³
@Temperature 390 °F
Hardened and tempered to 310 HB
 7.81 g/cc
@Temperature 20.0 °C
0.282 lb/in³
@Temperature 68.0 °F
Hardened and tempered to 310 HB
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 277 - 332277 - 332as supplied
 340
@Treatment Temp. 650 °C
340
@Treatment Temp. 1200 °F
Tempered for 2 hr
 380
@Treatment Temp. 600 °C
380
@Treatment Temp. 1110 °F
Tempered for 2 hr
Hardness, Rockwell C  45
@Treatment Temp. 500 °C
45
@Treatment Temp. 932 °F
Tempered for 2 hr
 47
@Treatment Temp. 400 °C
47
@Treatment Temp. 752 °F
Tempered for 2 hr
 49
@Treatment Temp. 300 °C
49
@Treatment Temp. 572 °F
Tempered for 2 hr
 52
@Treatment Temp. 180 °C
52
@Treatment Temp. 356 °F
Tempered for 2 hr
 52
@Treatment Temp. 200 °C
52
@Treatment Temp. 392 °F
Tempered for 2 hr
 55
@Treatment Temp. 300 °C
55
@Treatment Temp. 572 °F
Hardened for 2 hr, then Tempered
 59
@Treatment Temp. 200 °C
59
@Treatment Temp. 392 °F
Hardened for 2 hr, then Tempered
 60
@Treatment Temp. 180 °C
60
@Treatment Temp. 356 °F
Hardened for 2 hr, then Tempered
Hardness, Vickers  650
@Treatment Temp. 525 °C
650
@Treatment Temp. 977 °F
Nitriding in ammonia gas
 700
@Treatment Temp. 570 °C
700
@Treatment Temp. 1060 °F
Tufftriding (Tenifer process)
Tensile Strength, Ultimate  793 MPa
@Temperature 399 °C
115000 psi
@Temperature 750 °F
Round bar 1" diameter, 310 HB
 951 MPa
@Temperature 199 °C
138000 psi
@Temperature 390 °F
Round bar 1" diameter, 310 HB
 1010 MPa
@Temperature 20.0 °C
146000 psi
@Temperature 68.0 °F
Round bar 1" diameter, 310 HB
Tensile Strength, Yield  627 MPa
@Temperature 399 °C
91000 psi
@Temperature 750 °F
Round bar 1" diameter, 310 HB
 752 MPa
@Temperature 199 °C
109000 psi
@Temperature 390 °F
Round bar 1" diameter, 310 HB
 800 MPa
@Temperature 20.0 °C
116000 psi
@Temperature 68.0 °F
Round bar 1" diameter, 310 HB
Elongation at Yield  20 %
@Temperature 20.0 °C
20 %
@Temperature 68.0 °F
in 2"
 22 %
@Temperature 199 °C
22 %
@Temperature 390 °F
in 2"
 25 %
@Temperature 399 °C
25 %
@Temperature 750 °F
in 2"
Reduction of Area  60 %
@Temperature 20.0 °C
60 %
@Temperature 68.0 °F
 63 %
@Temperature 199 °C
63 %
@Temperature 390 °F
 65 %
@Temperature 399 °C
65 %
@Temperature 750 °F
Modulus of Elasticity  185 GPa
@Temperature 399 °C
26800 ksi
@Temperature 750 °F
 200 GPa
@Temperature 199 °C
29000 ksi
@Temperature 390 °F
 205 GPa
@Temperature 20.0 °C
29700 ksi
@Temperature 68.0 °F
Charpy Impact  50.2 J
@Temperature 20.0 °C
37.0 ft-lb
@Temperature 68.0 °F
Round bar 1" diameter, 310 HB
 55.6 J
@Temperature 199 °C
41.0 ft-lb
@Temperature 390 °F
Round bar 1" diameter, 310 HB
 65.1 J
@Temperature 399 °C
48.0 ft-lb
@Temperature 750 °F
Round bar 1" diameter, 310 HB
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.6 µm/m-°C
@Temperature 20.0 - 199 °C
7.00 µin/in-°F
@Temperature 68.0 - 390 °F
 13.5 µm/m-°C
@Temperature 20.0 - 399 °C
7.50 µin/in-°F
@Temperature 68.0 - 750 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 20.0 °C
0.110 BTU/lb-°F
@Temperature 68.0 °F
Thermal Conductivity  29.1 W/m-K
@Temperature 20.0 °C
202 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 29.5 W/m-K
@Temperature 199 °C
205 BTU-in/hr-ft²-°F
@Temperature 390 °F
 31.1 W/m-K
@Temperature 399 °C
216 BTU-in/hr-ft²-°F
@Temperature 750 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.31 %0.31 %
Chromium, Cr 1.2 %1.2 %
Iron, Fe 96.122 %96.122 %As Balance
Manganese, Mn 0.75 %0.75 %
Molybdenum, Mo 0.41 %0.41 %
Nickel, Ni 0.80 %0.80 %
Silicon, Si 0.40 %0.40 %
Sulfur, S 0.0080 %0.0080 %
 
Descriptive Properties
Color CodeOrange

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Bohler-Uddeholm P20 PREMIUM MODIFIED Pre-hardened Mold Steel
AISI Type P20 Mold Steel (UNS T51620)
Schmolz + Bickenbach P-20 High Hard Plastic Mold Steel
Schmolz + Bickenbach P-20 Modified Plastic Mold Steel
Bohler-Uddeholm IMPAX® P20 Hot Work Tool Steel

NSEDRO007 / 142944

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.