MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Elix Polymers Elix™ Ultra HH 4115 PG ABS Polymer
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Plating Grade

Material Notes: Very high heat resistance ABS plating grade. Extreme impact resistance with low temperature ductility, very high impact up to -30°C, well balanced flowability, heat resistance and flexibility, low emission and odor grade, lower mould deposits in injection molding processing applications, good dimensional precision, low shrinkage and CLTE. Main Applications: Household appliances, Housings (phone, computer, printer). Automotive interior, Automotive exterior, Toys, Cosmetics packaging, Extruded sheets, Medical devices, Electroplating, Pipes, Covers, Smart cards.

Property data measured at 23°C and 50% RH.

Information provided by Elix Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.07 g/cc0.0387 lb/in³ISO 1183-1
Linear Mold Shrinkage, Flow 0.0065 - 0.0075 cm/cm
@Thickness 2.00 mm
0.0065 - 0.0075 in/in
@Thickness 0.0787 in
60 X 60 mm; ISO-294-4
Linear Mold Shrinkage, Transverse 0.0065 - 0.0075 cm/cm
@Thickness 2.00 mm
0.0065 - 0.0075 in/in
@Thickness 0.0787 in
60 X 60 mm; ISO-294-4
Melt Flow 14 g/10 min
@Load 5.00 kg,
Temperature 260 °C
14 g/10 min
@Load 11.0 lb,
Temperature 500 °F
cm³/10 min MVR; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 90.0 MPa13100 psiISO 2039-1
Tensile Strength, Yield 42.0 MPa6090 psi50 mm/min; ISO 527-1,2
Elongation at Break >= 53 %>= 53 %50 mm/min; ISO 527-1,2
Elongation at Yield 7.0 %7.0 %50 mm/min; ISO 527-1,2
Tensile Modulus 2.00 GPa290 ksi1mm/min.; ISO 527-1,2
Flexural Strength 68.0 MPa9860 psi2mm/min; ISO 178
Flexural Modulus 2.00 GPa290 ksi2mm/min; ISO 178
Izod Impact, Notched (ISO)  41.0 kJ/m²
@Temperature -30.0 °C
19.5 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
 58.0 kJ/m²
@Temperature 23.0 °C
27.6 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
Charpy Impact, Notched  4.00 J/cm²
@Temperature -30.0 °C
19.0 ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eA
 5.30 J/cm²
@Temperature 23.0 °C
25.2 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 89.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
49.4 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,2
Deflection Temperature at 0.46 MPa (66 psi) 113 °C235 °FISO 75-1,2
Deflection Temperature at 1.8 MPa (264 psi) 101 °C214 °FISO 75-1,2
Vicat Softening Point 113 °C235 °FB50, 50°C/h; ISO 306
 115 °C239 °FB120, 120°C/h; ISO 306
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
Flammability Test >= 40
@Thickness 2.00 mm
>= 40
@Thickness 0.0787 in
US-FMVSS , mm/min; ISO 3795
 
Processing PropertiesMetricEnglishComments
Melt Temperature 240 °C464 °Finjection molding; ISO 294
Mold Temperature 70.0 °C158 °Finjection molding; ISO 294
Injection Velocity 240 mm/sec9.45 in/secinjection molding; ISO 294

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Elix Polymers ELIX PC/ABS 5130 Polycarbonate/ABS Alloy
Mitsubishi Iupilon® MB 8500 PC/ABS
Elix Polymers Elix™ Ultra HH 4115 HI ABS Polymer
Elix Polymers Elix™ 114 H ABS Polymer Modifier
Mitsubishi Iupilon® MB 8300 PC/ABS

PELIX923 / 192517

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.