MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Chevron Phillips Marlex® 9656 HDPE Blown Film Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Film Grade

Material Notes: Resin Type: high density, linear polyethylene.

Characteristics: copolymerization enhances film toughness, good drawdown, density level gives good machinability, blend well with LLDPE

Applications: notion and millinery bags, multi-wall liners, coextrusions

Recommended processing conditions: Die Gap 0.030-0.050 in. Melt Temperature 400°F.

Data provided by Chevron Phillips Chemical Company, LP.

Formerly branded with the MarFlex® trade name.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.956 g/cc0.0345 lb/in³ASTM D1505
Moisture Vapor Transmission 0.150 cc-mm/m²-24hr-atm0.381 cc-mil/100 in²-24hr-atmASTM F1249
Thickness 31.8 microns1.25 mil
Melt Flow 0.75 g/10 min0.75 g/10 minASTM D1238E
 
Mechanical PropertiesMetricEnglishComments
Film Elongation at Break, MD 580 %580 %ASTM D882
Film Elongation at Break, TD 500 %500 %ASTM D882
Elmendorf Tear Strength, MD 0.512 g/micron13.0 g/milNotched; ASTM D1922
Elmendorf Tear Strength, TD 23.6 g/micron600 g/milNotched; ASTM D1992
Dart Drop 1.97 g/micron50.0 g/milASTM D1709
Film Tensile Strength at Break, MD 51.0 MPa7400 psiASTM D882
Film Tensile Strength at Break, TD 17.9 MPa2600 psiASTM D882
1% Secant Modulus, MD 841 MPa122000 psiASTM D882
1% Secant Modulus, TD 1070 MPa155000 psiASTM D882
 
Processing PropertiesMetricEnglishComments
Processing Temperature 204 °C399 °F
Die Opening 0.0760 - 0.130 cm0.0299 - 0.0512 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Petrothene® LP510300 High Density Polyethylene
Chevron Phillips Marlex® 9659 HDPE Blown Film Resin
Chevron Phillips Marlex® 5755 LDPE High Clarity, High Impact Film Resin
LyondellBasell Petrothene® LR734001 High Density Polyethylene (Blow Molding Grade)
LyondellBasell Petrothene® LR734001 High Density Polyethylene, Sheet & Profile Extrusion Data

PCHEVVGO / 20568

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.