MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Henkel Loctite® Stycast® 2057M with CAT 28 Epoxy Encapsulant
Categories: Polymer; Thermoset; Epoxy; Epoxy Encapsulant, Unreinforced

Material Notes: Loctite Stycast 2057M provides the following product characteristics:
  • Low viscosity
  • Good machinability
  • General purpose
  • Rapid air release
  • Can be used with a variety of catalysts
  • Application: Encapsulation, Potting

Loctite Stycast 2057M is a general purpose encapsulant designed for machine dispensing and for parts requiring post molding machining. It contains a soft filler formulated to reduce abrasion in meter/mix equipment and to enhance machinability in the cured product.

Loctite Stycast 2057M can be used with a variety of catalysts.

CATALYST DESCRIPTION

Loctite CAT 28 provides the following product characteristics:

  • Long pot life
  • Excellent chemical resistance
  • Good physical and chemical properties at elevated temperatures

Cure: Heat cure

Information provided by Henkel.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccPart B, Loctite CAT 28
 1.74 g/ccPart A, Loctite Stycast 2057M
Water Absorption 0.14 %
@Temperature 100 °C,
Time 3600 sec
Cured
 0.020 %
@Time 86400 sec
Cured, RT
 0.090 %
@Time 605000 sec
7 Days at RT, Cured
Viscosity 275 cPPart B, Loctite CAT 28
Brookfield Viscosity 4.2 cPPart A, Loctite Stycast 2057M; Spindle 5, speed 50 rpm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 91
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 9.60e+15 ohm-cm
Surface Resistance 4.50e+16 ohm
Dielectric Constant 4.4
@Frequency 50 Hz
 4.5
@Frequency 1e+6 Hz
 4.7
@Frequency 1000 Hz
Dissipation Factor 0.0040
@Frequency 1000 Hz
 0.0050
@Frequency 50 Hz
 0.022
@Frequency 1e+6 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 51.0 µm/m-°C
@Temperature <=83.0 °C
Below Tg; TMA
 132 µm/m-°C
@Temperature >=83.0 °C
Above Tg; TMA
Maximum Service Temperature, Air 175 °CContinuous
 200 °CIntermittent
Minimum Service Temperature, Air -40.0 °CContinuous
 -40.0 °CIntermittent
Glass Transition Temp, Tg 83.0 °CTMA
 94.0 °CDMA, @ onset point
 114 °CDMA, tan delta
 
Processing PropertiesOriginal ValueComments
Cure Time 4.00 hour
@Temperature 120 °C
Shelf Life 12.0 MonthPart A, Loctite Stycast 2057M
 
Descriptive Properties
AppearanceBlackPart A, Loctite Stycast 2057M
Mix Ratio, by Weight100 : 7Material : Catalyst

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHENK7915 / 255402

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.