MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow NRD6-589 Polypropylene Random Copolymer Resin  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer; Polypropylene, Impact Modified; Molded/Extruded; Polypropylene, Molded

Material Notes: DOW NRD6-589 Polypropylene Resin is intended for use in injection molding applications. It offers excellent balance of impact and stiffness.

  • Consistent processability
  • Good stiffness/impact balance
  • Good contact clarity
  • Contains nucleating additive
  • Contains an antistatic additive

    Complies with
  • U.S. FDA 21 CFR 177.1520 (c)3.2a
  • Canadian HPFB No Objection
  • U.S. FDA-DMF
  • Europe EU-Directive 2002/72/EC

Braskem acquired Dow's polypropylene business. This specific grade was discontinued priot to the acquisition and so is listed as a discontinued Dow product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ASTM D792
Melt Index of Compound 35 g/10 min
@Load 2.16 kg,
Temperature 230 °C
35 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 106106ASTM D785
Tensile Strength, Yield 35.2 MPa5110 psiASTM D638
Elongation at Yield 7.0 %7.0 %ASTM D638
Flexural Modulus, 1% Secant 1380 MPa200000 psiASTM D790A
Izod Impact, Notched 0.374 J/cm0.701 ft-lb/inASTM D256A
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 102 °C216 °FUnannealed; ASTM D648
Vicat Softening Point 150 °C302 °FASTM D1525
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow R792-35RNA Polypropylene Random Copolymer Resin
Dow 6D43 Polypropylene Random Copolymer Resin
CTC X-PRO CTC PP 3020 Polypropylene Copolymer
CTC X-PRO CTC PP 2040 Polypropylene Copolymer
Dow 6D20 Polypropylene Random Copolymer Resin

PDOW0980 / 93316

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.