MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Celanex® 2000-2 PBT, Unfilled
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: Celanex 2000-2 is a general purpose, unreinforced polybutylene terephthalate with a good balance of mechanical properties and processability. Celanex 2000-2 is a high flow material that contains an internal lubricant.
To avoid hydrolytic degradation during processing, CELANEX resins have to be dried to a moisture level equal to or less than 0.02%. Drying should be done in a dehumidifying hopper dryer capable of dew points <-40°F (-40°C) at 250°F (121°C) for 4 hours.
For subsequent storage of the material in the dryer until processed (<= 60 h) it is necessary to lower the temperature to 100° C.

Information provided by Celanese Corporation.

Key Words: High melt flow, lubricated
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.31 g/cc1.31 g/ccASTM D792
Density 1.31 g/cc0.0473 lb/in³ISO 1183
Water Absorption 0.090 %
@Temperature 22.8 °C
0.090 %
@Temperature 73.0 °F
24hr immersion; ASTM D570
Viscosity Test 75 cm³/g0.75 dl/gISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.018 - 0.020 cm/cm0.018 - 0.020 in/inASTM D955
 0.018 - 0.020 cm/cm0.018 - 0.020 in/inISO 294-4
Melt Flow 65 g/10 min65 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7575ISO 2039-2
Tensile Strength, Yield 60.0 MPa8700 psi50mm/min; ISO 527-2/1A
 57.2 MPa
@Temperature 22.8 °C
8300 psi
@Temperature 73.0 °F
ASTM D638
Tensile Stress at Strain  8.62 MPa
@Strain 0.32 %,
Temperature 23.0 °C
1250 psi
@Strain 0.32 %,
Temperature 73.4 °F
 16.8 MPa
@Strain 0.64 %,
Temperature 23.0 °C
2440 psi
@Strain 0.64 %,
Temperature 73.4 °F
 24.6 MPa
@Strain 0.96 %,
Temperature 23.0 °C
3570 psi
@Strain 0.96 %,
Temperature 73.4 °F
 31.8 MPa
@Strain 1.28 %,
Temperature 23.0 °C
4610 psi
@Strain 1.28 %,
Temperature 73.4 °F
 38.2 MPa
@Strain 1.6 %,
Temperature 23.0 °C
5540 psi
@Strain 1.6 %,
Temperature 73.4 °F
 43.6 MPa
@Strain 1.92 %,
Temperature 23.0 °C
6320 psi
@Strain 1.92 %,
Temperature 73.4 °F
 47.6 MPa
@Strain 2.24 %,
Temperature 23.0 °C
6900 psi
@Strain 2.24 %,
Temperature 73.4 °F
 49.8 MPa
@Strain 2.56 %,
Temperature 23.0 °C
7220 psi
@Strain 2.56 %,
Temperature 73.4 °F
 50.8 MPa
@Strain 2.88 %,
Temperature 23.0 °C
7370 psi
@Strain 2.88 %,
Temperature 73.4 °F
 51.1 MPa
@Strain 3.2 %,
Temperature 23.0 °C
7410 psi
@Strain 3.2 %,
Temperature 73.4 °F
Elongation at Break 30 %30 %50mm/min; ISO 527-2/1A
 5.0 %
@Temperature 22.8 °C
5.0 %
@Temperature 73.0 °F
ASTM D638
Elongation at Yield 4.0 %4.0 %50mm/min; ISO 527-2/1A
Tensile Modulus 2.70 GPa392 ksi1mm/min; ISO 527-2/1A
Flexural Strength 85.0 MPa12300 psiISO 178
 85.5 MPa
@Temperature 22.8 °C
12400 psi
@Temperature 73.0 °F
ASTM D790
Flexural Modulus 2.60 GPa377 ksiISO 178
 2.48 GPa
@Temperature 22.8 °C
360 ksi
@Temperature 73.0 °F
ASTM D790
Shear Modulus  0.0181 GPa
@Temperature 220 °C
2.63 ksi
@Temperature 428 °F
 0.0380 GPa
@Temperature 210 °C
5.51 ksi
@Temperature 410 °F
 0.0481 GPa
@Temperature 200 °C
6.98 ksi
@Temperature 392 °F
 0.0552 GPa
@Temperature 190 °C
8.01 ksi
@Temperature 374 °F
 0.0623 GPa
@Temperature 180 °C
9.04 ksi
@Temperature 356 °F
 0.0682 GPa
@Temperature 170 °C
9.89 ksi
@Temperature 338 °F
 0.0739 GPa
@Temperature 160 °C
10.7 ksi
@Temperature 320 °F
 0.0796 GPa
@Temperature 150 °C
11.5 ksi
@Temperature 302 °F
 0.0861 GPa
@Temperature 140 °C
12.5 ksi
@Temperature 284 °F
 0.0935 GPa
@Temperature 130 °C
13.6 ksi
@Temperature 266 °F
 0.101 GPa
@Temperature 120 °C
14.6 ksi
@Temperature 248 °F
 0.111 GPa
@Temperature 110 °C
16.1 ksi
@Temperature 230 °F
 0.122 GPa
@Temperature 100 °C
17.7 ksi
@Temperature 212 °F
 0.139 GPa
@Temperature 90.0 °C
20.2 ksi
@Temperature 194 °F
 0.168 GPa
@Temperature 80.0 °C
24.4 ksi
@Temperature 176 °F
 0.220 GPa
@Temperature 70.0 °C
31.9 ksi
@Temperature 158 °F
 0.334 GPa
@Temperature 60.0 °C
48.4 ksi
@Temperature 140 °F
 0.572 GPa
@Temperature 50.0 °C
83.0 ksi
@Temperature 122 °F
 0.734 GPa
@Temperature 40.0 °C
106 ksi
@Temperature 104 °F
 0.773 GPa
@Temperature 30.0 °C
112 ksi
@Temperature 86.0 °F
 0.797 GPa
@Temperature 23.0 °C
116 ksi
@Temperature 73.4 °F
 0.832 GPa
@Temperature 10.0 °C
121 ksi
@Temperature 50.0 °F
 0.855 GPa
@Temperature 0.000 °C
124 ksi
@Temperature 32.0 °F
 0.879 GPa
@Temperature -10.0 °C
127 ksi
@Temperature 14.0 °F
 0.904 GPa
@Temperature -20.0 °C
131 ksi
@Temperature -4.00 °F
 0.930 GPa
@Temperature -30.0 °C
135 ksi
@Temperature -22.0 °F
 0.961 GPa
@Temperature -40.0 °C
139 ksi
@Temperature -40.0 °F
 0.986 GPa
@Temperature -50.0 °C
143 ksi
@Temperature -58.0 °F
 1.07 GPa
@Temperature -60.0 °C
155 ksi
@Temperature -76.0 °F
Izod Impact, Notched 0.374 J/cm
@Temperature 22.8 °C
0.700 ft-lb/in
@Temperature 73.0 °F
ASTM D256
Izod Impact, Notched (ISO) 3.20 kJ/m²1.52 ft-lb/in²ISO 180/1A
Charpy Impact Unnotched 10.0 J/cm²47.6 ft-lb/in²ISO 179/1eU
 9.00 J/cm²
@Temperature -30.0 °C
42.8 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.400 J/cm²1.90 ft-lb/in²ISO 179/1eA
 0.350 J/cm²
@Temperature -30.0 °C
1.67 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cmIEC 60093
 1.00e+16 ohm-cm1.00e+16 ohm-cmASTM D257
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant  3.2
@Frequency 1e+6 Hz
3.2
@Frequency 1e+6 Hz
ASTM D150
 3.5
@Frequency 1e+6 Hz
3.5
@Frequency 1e+6 Hz
IEC 60250
 4.0
@Frequency 100 Hz
4.0
@Frequency 100 Hz
IEC 60250
Dielectric Strength 16.5 kV/mm420 kV/inshort term; ASTM D149
 23.0 kV/mm584 kV/inIEC 60243-1
Dissipation Factor  0.0015
@Frequency 100 Hz
0.0015
@Frequency 100 Hz
IEC 60250
 0.0020
@Frequency 1e+6 Hz
0.0020
@Frequency 1e+6 Hz
ASTM D150
 0.020
@Frequency 1e+6 Hz
0.020
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C61.1 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 86.0 µm/m-°C47.8 µin/in-°FISO 11359-2
Melting Point 225 °C437 °FISO 11357-1,-2,-3
 225 °C437 °FASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 155 °C311 °FISO 75-1, -2
 162 °C324 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 50.6 °C123 °FASTM D648
 55.0 °C131 °FISO 75-1, -2
Vicat Softening Point 190 °C374 °FB50 (50°C/h 50N); ISO 306
Glass Transition Temp, Tg 60.0 °C140 °FISO 11357-1,-2,-3
Flammability, UL94 HB
@Thickness 0.710 mm
HB
@Thickness 0.0280 in
Oxygen Index 22 %22 %ISO 4589
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 50.0 °C68.0 - 122 °Fhopper
 65.0 - 93.0 °C149 - 199 °Fcavity
Feed Temperature 230 - 240 °C446 - 464 °F
Zone 1 230 - 240 °C446 - 464 °F
Zone 2 235 - 250 °C455 - 482 °F
Zone 3 235 - 250 °C455 - 482 °F
Zone 4 240 - 260 °C464 - 500 °F
Die Temperature 250 - 260 °C482 - 500 °F
Melt Temperature 243 °C469 °FISO 294
 235 - 260 °C455 - 500 °F
Mold Temperature 82.0 °C180 °FISO 294
Injection Velocity 300 mm/sec11.8 in/secISO 294
Drying Temperature 120 - 130 °C248 - 266 °F
Dry Time 4 hour4 hour
Moisture Content 0.020 %0.020 %Necessary low maximum
Injection Pressure 48.0 MPa6960 psiISO 294
Hot-Working Temperature 250 - 260 °C482 - 500 °F
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast
Processing conditions acc. ISO7792-2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Celanex® 1300A Polyester (PBT)
Overview of materials for Polycarbonate/Polybutylene Terephthalate (PBT) Blend, Unreinforced
Overview of materials for Polybutylene Terephthalate (PBT), Impact Grade
Overview of materials for Polybutylene Terephthalate (PBT), Flame Retardant
Overview of materials for Polybutylene Terephthalate (PBT), Extrusion Grade

PHCS009 / 123424

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.