MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

(Viewing data as-entered. Click here to return)
Eastman Eastar MN211 Copolyester, Natural
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: Product Description: Meets ISO 10993 and/or USP Class VI biocompatibility requirement. Eastar™ Copolyester MN211, Natural contains a mold release for imp roved ejection. It is a brilliantly clear polymer with good impact strength, chemical resistance, dimensional stability, and low shrinkage rates. The slower rate of crystallization of this material makes it excellent for use in hot runner systems with valve or thermal gates. This product has been GREENGUARD INDOOR AIR QUALITY CERTIFIED

Applications/Uses:

  • Blood Contact
  • Drug Delivery
  • IV Components
  • Medical
  • Surgical Instruments
Key Attributes:
  • Chemical resistance to most medical solvents including lipids and IPA
  • Gamma and E-beam color stability

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.27 g/ccASTM D792
Water Absorption 0.13 %24h Immersion; ASTM D570
Linear Mold Shrinkage 0.0020 - 0.0050 cm/cm
@Thickness 3.20 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 106ASTM D785
Tensile Strength at Break 28.0 MPaASTM D638
Tensile Strength, Yield 50.0 MPaASTM D638
Elongation at Break 110 %ASTM D638
Elongation at Yield 4.3 %ASTM D638
Flexural Strength 70.0 MPaASTM D790
Flexural Modulus 2.10 GPaASTM D790
Izod Impact, Notched 0.370 J/cm
@Temperature -40.0 °C
ASTM D256
 101 J/m
@Temperature 23.0 °C
ASTM D256
Izod Impact, Unnotched NBASTM D4812
 NB
@Temperature -40.0 °C
ASTM D4812
 
Thermal PropertiesOriginal ValueComments
Specific Heat Capacity 1.30 J/g-°C
@Temperature 60.0 °C
DSC
 2.01 J/g-°C
@Temperature 240 °C
DSC
Thermal Conductivity 0.190 W/m-KASTM C177
Deflection Temperature at 0.46 MPa (66 psi) 70.0 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 63.0 °CASTM D648
Vicat Softening Point 85.0 °C1kg load; ASTM D1525
 
Optical PropertiesOriginal ValueComments
Haze 0.30 %ASTM D1003
Transmission, Visible 88 %Regular Transmittance; ASTM D1003
 91 %Total Transmittance; ASTM D1003
 
Processing PropertiesOriginal ValueComments
Melt Temperature 249 - 271 °C
Mold Temperature 16.0 - 38.0 °C
Drying Temperature 71.0 °C
Dry Time 4 - 6 hour
 
Compliance PropertiesOriginal ValueComments
USP Class VI Yes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Eastman Tritan™ MX711 Medical Grade Copolyester
Eastman DuraStar DS1000 Polymer, Natural
Eastman DuraStar DS1900HF Polymer, Natural
Eastman Eastar 6763 PETG Copolyester
Eastman Tritan™ MX811 Medical Grade Copolyester

PE9056 / 35112

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.