MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2219-T851 (Extended High Temperature Data)
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
This designation is considered the sole original alloy for this alloy family.
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92219; ISO AlCu6Mn; Aluminium 2219-T851; AA2219-T851
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.84 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 130500 kg load with 10 mm ball
Hardness, Knoop 163Converted from Brinell Hardness Value
Hardness, Rockwell A 49.5Converted from Brinell Hardness Value
Hardness, Rockwell B 80Converted from Brinell Hardness Value
Hardness, Vickers 149Converted from Brinell Hardness Value
Tensile Strength, Ultimate 66.0 ksiAA; Typical
 >= 400 MPaWire, rod, bar, and shapes (extruded); T8510, T8511
 >= 400 MPaExtruded tube; T8510, T8511
 30.0 MPa
@Temperature 371 °C
 48.0 MPa
@Temperature 316 °C
 200 MPa
@Temperature 260 °C
 248 MPa
@Temperature 204 °C
 338 MPa
@Temperature 149 °C
 414 MPa
@Temperature 100 °C
 455 MPa
@Temperature 24.0 °C
 476 MPa
@Temperature -28.0 °C
 490 MPa
@Temperature -80.0 °C
 572 MPa
@Temperature -196 °C
 >= 395 MPa
@Thickness 127.0 - 152 mm
Plate
 >= 405 MPa
@Thickness 101.6 - 127 mm
Plate
 >= 415 MPa
@Thickness 76.23 - 102 mm
Plate
 >= 425 MPa
@Thickness 6.35 - 50.8 mm
Plate
 >= 425 MPa
@Thickness 50.83 - 76.2 mm
Plate
 >= 395 MPa
@Diameter 50.83 - 102 mm
Wire, rod, and bar (rolled or cold finished)
 >= 400 MPa
@Diameter 12.7 - 50.8 mm
Wire, rod, and bar (rolled or cold finished)
Tensile Strength, Yield 51.0 ksiAA; Typical
 >= 290 MPaWire, rod, bar, and shapes (extruded); T8510, T8511
 >= 290 MPaExtruded tube; T8510, T8511
 >= 290 MPa
@Thickness 127.0 - 152 mm
Plate
 >= 295 MPa
@Thickness 101.6 - 127 mm
Plate
 >= 305 MPa
@Thickness 76.23 - 102 mm
Plate
 >= 310 MPa
@Thickness 50.83 - 76.2 mm
Plate
 >= 315 MPa
@Thickness 6.35 - 50.8 mm
Plate
 >= 270 MPa
@Diameter 50.83 - 102 mm
Wire, rod, and bar (rolled or cold finished)
 >= 275 MPa
@Diameter 12.7 - 50.8 mm
Wire, rod, and bar (rolled or cold finished)
 26.0 MPa
@Strain 0.2 %,
Temperature 371 °C
 41.0 MPa
@Strain 0.2 %,
Temperature 316 °C
 159 MPa
@Strain 0.2 %,
Temperature 260 °C
 200 MPa
@Strain 0.2 %,
Temperature 204 °C
 276 MPa
@Strain 0.2 %,
Temperature 149 °C
 324 MPa
@Strain 0.2 %,
Temperature 100 °C
 345 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 359 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 372 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 421 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 6.0 %Wire, rod, bar, and shapes (extruded); T8510, T8511
 6.0 %Extruded tube; T8510, T8511
 12 %
@Temperature -28.0 °C
 12 %
@Temperature 24.0 °C
 13 %
@Temperature -80.0 °C
 15 %
@Temperature -196 °C
 15 %
@Temperature 100 °C
 17 %
@Temperature 149 °C
 20 %
@Temperature 204 °C
 21 %
@Temperature 260 °C
 55 %
@Temperature 316 °C
 75 %
@Temperature 371 °C
 4.0 %
@Thickness 127.0 - 152 mm
Plate
 5.0 %
@Thickness 76.23 - 102 mm
Plate
 5.0 %
@Thickness 101.6 - 127 mm
Plate
 6.0 %
@Thickness 50.83 - 76.2 mm
Plate
 7.0 - 8.0 %
@Thickness 6.35 - 50.8 mm
Plate
 10 %
@Thickness 1.59 mm
AA; Typical
 4.0 %
@Diameter 12.7 - 50.8 mm
Wire, rod, and bar (rolled or cold finished)
 4.0 %
@Diameter 50.83 - 102 mm
Wire, rod, and bar (rolled or cold finished)
Creep Strength 11.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
0.5% creep
 13.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
1% creep
 13.0 MPa
@Temperature 370 °C,
Time 360000 sec
0.2% creep
 18.0 MPa
@Temperature 370 °C,
Time 360000 sec
0.5% creep
 18.0 MPa
@Temperature 370 °C,
Time 36000 sec
0.1% creep
 20.0 MPa
@Temperature 370 °C,
Time 360000 sec
1% creep
 23.0 MPa
@Temperature 370 °C,
Time 36000 sec
0.2% creep
 23.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
0.1% creep
 27.0 MPa
@Temperature 370 °C,
Time 36000 sec
0.5% creep
 28.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
0.2% creep
 30.0 MPa
@Temperature 370 °C,
Time 36000 sec
1% creep
 32.0 MPa
@Temperature 370 °C,
Time 3600 sec
0.1% creep
 38.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
0.5% creep
 38.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.1% creep
 41.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
1% creep
 45.0 MPa
@Temperature 370 °C,
Time 3600 sec
0.2% creep
 52.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.2% creep
 59.0 MPa
@Temperature 370 °C,
Time 3600 sec
0.5% creep
 59.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
0.1% creep
 62.0 MPa
@Temperature 370 °C,
Time 3600 sec
1% creep
 62.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.5% creep
 62.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.1% creep
 66.0 MPa
@Temperature 370 °C,
Time 360 sec
0.2% creep
 66.0 MPa
@Temperature 370 °C,
Time 360 sec
0.1% creep
 69.0 MPa
@Temperature 260 °C,
Time 360000 sec
0.1% creep
 69.0 MPa
@Temperature 260 °C,
Time 3.60e+7 sec
1% creep
 69.0 MPa
@Temperature 315 °C,
Time 360000 sec
1% creep
 69.0 MPa
@Temperature 370 °C,
Time 360 sec
1% creep
 69.0 MPa
@Temperature 370 °C,
Time 360 sec
0.5% creep
 69.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
0.2% creep
 69.0 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
0.1% creep
 76.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.2% creep
 83.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
0.5% creep
 90.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.5% creep
 90.0 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
0.2% creep
 90.0 MPa
@Temperature 260 °C,
Time 360000 sec
0.2% creep
 90.0 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.1% creep
 90.0 MPa
@Temperature 230 °C,
Time 360000 sec
0.1% creep
 90.0 MPa
@Temperature 260 °C,
Time 36000 sec
0.1% creep
 90.0 MPa
@Temperature 315 °C,
Time 3600 sec
0.1% creep
 97.0 MPa
@Temperature 230 °C,
Time 3.60e+7 sec
1% creep
 97.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
1% creep
 97.0 MPa
@Temperature 315 °C,
Time 36000 sec
1% creep
 97.0 MPa
@Temperature 230 °C,
Time 3.60e+7 sec
0.5% creep
 105 MPa
@Temperature 315 °C,
Time 3600 sec
0.2% creep
 105 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
0.1% creep
 110 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
0.5% creep
 110 MPa
@Temperature 260 °C,
Time 360000 sec
0.5% creep
 110 MPa
@Temperature 315 °C,
Time 3600 sec
0.5% creep
 110 MPa
@Temperature 230 °C,
Time 360000 sec
0.2% creep
 110 MPa
@Temperature 260 °C,
Time 36000 sec
0.2% creep
 110 MPa
@Temperature 205 °C,
Time 360000 sec
0.1% creep
 110 MPa
@Temperature 230 °C,
Time 36000 sec
0.1% creep
 110 MPa
@Temperature 315 °C,
Time 360 sec
0.1% creep
 115 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
1% creep
 115 MPa
@Temperature 315 °C,
Time 3600 sec
1% creep
 115 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.2% creep
 115 MPa
@Temperature 315 °C,
Time 360 sec
0.2% creep
 115 MPa
@Temperature 260 °C,
Time 3600 sec
0.1% creep
 125 MPa
@Temperature 205 °C,
Time 3.60e+7 sec
1% creep
 125 MPa
@Temperature 260 °C,
Time 360000 sec
1% creep
 125 MPa
@Temperature 315 °C,
Time 360 sec
1% creep
 125 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.5% creep
 125 MPa
@Temperature 315 °C,
Time 360 sec
0.5% creep
 130 MPa
@Temperature 230 °C,
Time 360000 sec
0.5% creep
 130 MPa
@Temperature 260 °C,
Time 36000 sec
0.5% creep
 130 MPa
@Temperature 205 °C,
Time 360000 sec
0.2% creep
 130 MPa
@Temperature 230 °C,
Time 36000 sec
0.2% creep
 130 MPa
@Temperature 175 °C,
Time 360000 sec
0.1% creep
 130 MPa
@Temperature 205 °C,
Time 36000 sec
0.1% creep
 140 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
1% creep
 140 MPa
@Temperature 230 °C,
Time 360000 sec
1% creep
 140 MPa
@Temperature 260 °C,
Time 36000 sec
1% creep
 140 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
0.2% creep
 140 MPa
@Temperature 260 °C,
Time 3600 sec
0.2% creep
 140 MPa
@Temperature 230 °C,
Time 3600 sec
0.1% creep
 145 MPa
@Temperature 260 °C,
Time 360 sec
0.1% creep
 150 MPa
@Temperature 205 °C,
Time 360000 sec
0.5% creep
 150 MPa
@Temperature 230 °C,
Time 36000 sec
0.5% creep
 150 MPa
@Temperature 260 °C,
Time 3600 sec
0.5% creep
 150 MPa
@Temperature 205 °C,
Time 36000 sec
0.2% creep
 150 MPa
@Temperature 230 °C,
Time 3600 sec
0.2% creep
 150 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.1% creep
 160 MPa
@Temperature 230 °C,
Time 36000 sec
1% creep
 160 MPa
@Temperature 260 °C,
Time 3600 sec
1% creep
 160 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
0.5% creep
 160 MPa
@Temperature 175 °C,
Time 360000 sec
0.2% creep
 160 MPa
@Temperature 260 °C,
Time 360 sec
0.2% creep
 160 MPa
@Temperature 205 °C,
Time 3600 sec
0.1% creep
 165 MPa
@Temperature 205 °C,
Time 360000 sec
1% creep
 165 MPa
@Temperature 260 °C,
Time 360 sec
0.5% creep
 165 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.2% creep
 165 MPa
@Temperature 175 °C,
Time 36000 sec
0.1% creep
 165 MPa
@Temperature 230 °C,
Time 360 sec
0.1% creep
 170 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
1% creep
 170 MPa
@Temperature 260 °C,
Time 360 sec
1% creep
 170 MPa
@Temperature 230 °C,
Time 3600 sec
0.5% creep
 170 MPa
@Temperature 150 °C,
Time 360000 sec
0.1% creep
 180 MPa
@Temperature 205 °C,
Time 36000 sec
0.5% creep
 180 MPa
@Temperature 205 °C,
Time 3600 sec
0.2% creep
 180 MPa
@Temperature 230 °C,
Time 360 sec
0.2% creep
 185 MPa
@Temperature 230 °C,
Time 3600 sec
1% creep
 185 MPa
@Temperature 175 °C,
Time 360000 sec
0.5% creep
 195 MPa
@Temperature 205 °C,
Time 36000 sec
1% creep
 195 MPa
@Temperature 175 °C,
Time 36000 sec
0.2% creep
 195 MPa
@Temperature 205 °C,
Time 360 sec
0.1% creep
 200 MPa
@Temperature 175 °C,
Time 360000 sec
1% creep
 200 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.5% creep
 200 MPa
@Temperature 230 °C,
Time 360 sec
0.5% creep
 200 MPa
@Temperature 150 °C,
Time 360000 sec
0.2% creep
 200 MPa
@Temperature 175 °C,
Time 3600 sec
0.1% creep
 205 MPa
@Temperature 230 °C,
Time 360 sec
1% creep
 205 MPa
@Temperature 205 °C,
Time 3600 sec
0.5% creep
 205 MPa
@Temperature 150 °C,
Time 36000 sec
0.1% creep
 215 MPa
@Temperature 175 °C,
Time 36000 sec
0.5% creep
 215 MPa
@Temperature 205 °C,
Time 360 sec
0.2% creep
 220 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
1% creep
 220 MPa
@Temperature 205 °C,
Time 3600 sec
1% creep
 220 MPa
@Temperature 175 °C,
Time 3600 sec
0.2% creep
 230 MPa
@Temperature 175 °C,
Time 36000 sec
1% creep
 230 MPa
@Temperature 175 °C,
Time 360 sec
0.1% creep
 235 MPa
@Temperature 150 °C,
Time 360000 sec
0.5% creep
 235 MPa
@Temperature 205 °C,
Time 360 sec
0.5% creep
 235 MPa
@Temperature 150 °C,
Time 36000 sec
0.2% creep
 235 MPa
@Temperature 150 °C,
Time 3600 sec
0.1% creep
 240 MPa
@Temperature 205 °C,
Time 360 sec
1% creep
 240 MPa
@Temperature 175 °C,
Time 3600 sec
0.5% creep
 250 MPa
@Temperature 150 °C,
Time 360000 sec
1% creep
 250 MPa
@Temperature 175 °C,
Time 360 sec
0.2% creep
 255 MPa
@Temperature 175 °C,
Time 3600 sec
1% creep
 255 MPa
@Temperature 150 °C,
Time 36000 sec
0.5% creep
 255 MPa
@Temperature 150 °C,
Time 3600 sec
0.2% creep
 260 MPa
@Temperature 175 °C,
Time 360 sec
0.5% creep
 260 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
0.1% creep
 260 MPa
@Temperature 150 °C,
Time 360 sec
0.1% creep
 270 MPa
@Temperature 150 °C,
Time 36000 sec
1% creep
 270 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
0.2% creep
 270 MPa
@Temperature 100 °C,
Time 360000 sec
0.1% creep
 275 MPa
@Temperature 175 °C,
Time 360 sec
1% creep
 275 MPa
@Temperature 150 °C,
Time 3600 sec
0.5% creep
 275 MPa
@Temperature 100 °C,
Time 360000 sec
0.2% creep
 275 MPa
@Temperature 150 °C,
Time 360 sec
0.2% creep
 275 MPa
@Temperature 100 °C,
Time 36000 sec
0.1% creep
 285 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
0.5% creep
 285 MPa
@Temperature 100 °C,
Time 3600 sec
0.1% creep
 290 MPa
@Temperature 150 °C,
Time 3600 sec
1% creep
 290 MPa
@Temperature 100 °C,
Time 36000 sec
0.2% creep
 295 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
1% creep
 295 MPa
@Temperature 100 °C,
Time 360000 sec
0.5% creep
 295 MPa
@Temperature 150 °C,
Time 360 sec
0.5% creep
 305 MPa
@Temperature 150 °C,
Time 360 sec
1% creep
 305 MPa
@Temperature 100 °C,
Time 3600 sec
0.2% creep
 305 MPa
@Temperature 100 °C,
Time 360 sec
0.1% creep
 310 MPa
@Temperature 100 °C,
Time 360000 sec
1% creep
 310 MPa
@Temperature 100 °C,
Time 36000 sec
0.5% creep
 315 MPa
@Temperature 100 °C,
Time 360 sec
0.2% creep
 315 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
0.1% creep
 325 MPa
@Temperature 100 °C,
Time 36000 sec
1% creep
 325 MPa
@Temperature 100 °C,
Time 3600 sec
0.5% creep
 325 MPa
@Temperature 24.0 °C,
Time 360000 sec
0.1% creep
 330 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
0.2% creep
 330 MPa
@Temperature 24.0 °C,
Time 36000 sec
0.1% creep
 340 MPa
@Temperature 100 °C,
Time 3600 sec
1% creep
 340 MPa
@Temperature 100 °C,
Time 360 sec
0.5% creep
 340 MPa
@Temperature 24.0 °C,
Time 360000 sec
0.2% creep
 345 MPa
@Temperature 24.0 °C,
Time 36000 sec
0.2% creep
 345 MPa
@Temperature 24.0 °C,
Time 3600 sec
0.1% creep
 350 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
0.5% creep
 350 MPa
@Temperature 24.0 °C,
Time 360 sec
0.1% creep
 360 MPa
@Temperature 100 °C,
Time 360 sec
1% creep
 360 MPa
@Temperature 24.0 °C,
Time 360000 sec
0.5% creep
 360 MPa
@Temperature 24.0 °C,
Time 3600 sec
0.2% creep
 365 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
1% creep
 365 MPa
@Temperature 24.0 °C,
Time 36000 sec
0.5% creep
 365 MPa
@Temperature 24.0 °C,
Time 360 sec
0.2% creep
 380 MPa
@Temperature 24.0 °C,
Time 360000 sec
1% creep
 385 MPa
@Temperature 24.0 °C,
Time 3600 sec
0.5% creep
 400 MPa
@Temperature 24.0 °C,
Time 36000 sec
1% creep
 415 MPa
@Temperature 24.0 °C,
Time 360 sec
0.5% creep
 420 MPa
@Temperature 24.0 °C,
Time 3600 sec
1% creep
 435 MPa
@Temperature 24.0 °C,
Time 360 sec
1% creep
Rupture Strength 14.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
 22.0 MPa
@Temperature 315 °C,
Time 3.60e+7 sec
 22.0 MPa
@Temperature 370 °C,
Time 360000 sec
 32.0 MPa
@Temperature 370 °C,
Time 36000 sec
 41.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
 45.0 MPa
@Temperature 260 °C,
Time 3.60e+8 sec
 62.0 MPa
@Temperature 370 °C,
Time 3600 sec
 66.0 MPa
@Temperature 230 °C,
Time 3.60e+8 sec
 69.0 MPa
@Temperature 260 °C,
Time 3.60e+7 sec
 69.0 MPa
@Temperature 315 °C,
Time 360000 sec
 69.0 MPa
@Temperature 370 °C,
Time 360 sec
 97.0 MPa
@Temperature 205 °C,
Time 3.60e+8 sec
 97.0 MPa
@Temperature 230 °C,
Time 3.60e+7 sec
 105 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
 105 MPa
@Temperature 315 °C,
Time 36000 sec
 115 MPa
@Temperature 315 °C,
Time 3600 sec
 125 MPa
@Temperature 205 °C,
Time 3.60e+7 sec
 125 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
 130 MPa
@Temperature 175 °C,
Time 3.60e+8 sec
 130 MPa
@Temperature 260 °C,
Time 360000 sec
 130 MPa
@Temperature 315 °C,
Time 360 sec
 150 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
 150 MPa
@Temperature 230 °C,
Time 360000 sec
 150 MPa
@Temperature 260 °C,
Time 36000 sec
 160 MPa
@Temperature 175 °C,
Time 3.60e+7 sec
 165 MPa
@Temperature 260 °C,
Time 3600 sec
 170 MPa
@Temperature 150 °C,
Time 3.60e+8 sec
 170 MPa
@Temperature 230 °C,
Time 36000 sec
 180 MPa
@Temperature 205 °C,
Time 360000 sec
 180 MPa
@Temperature 260 °C,
Time 360 sec
 185 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
 200 MPa
@Temperature 230 °C,
Time 3600 sec
 205 MPa
@Temperature 150 °C,
Time 3.60e+7 sec
 205 MPa
@Temperature 205 °C,
Time 36000 sec
 220 MPa
@Temperature 175 °C,
Time 360000 sec
 230 MPa
@Temperature 230 °C,
Time 360 sec
 235 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
 235 MPa
@Temperature 205 °C,
Time 3600 sec
 250 MPa
@Temperature 175 °C,
Time 36000 sec
 260 MPa
@Temperature 150 °C,
Time 360000 sec
 270 MPa
@Temperature 205 °C,
Time 360 sec
 275 MPa
@Temperature 175 °C,
Time 3600 sec
 290 MPa
@Temperature 150 °C,
Time 36000 sec
 305 MPa
@Temperature 175 °C,
Time 360 sec
 315 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
 315 MPa
@Temperature 150 °C,
Time 3600 sec
 330 MPa
@Temperature 100 °C,
Time 360000 sec
 340 MPa
@Temperature 150 °C,
Time 360 sec
 350 MPa
@Temperature 100 °C,
Time 36000 sec
 370 MPa
@Temperature 100 °C,
Time 3600 sec
 395 MPa
@Temperature 100 °C,
Time 360 sec
 420 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
 425 MPa
@Temperature 24.0 °C,
Time 360000 sec
 435 MPa
@Temperature 24.0 °C,
Time 36000 sec
 450 MPa
@Temperature 24.0 °C,
Time 3600 sec
 455 MPa
@Temperature 24.0 °C,
Time 360 sec
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 15000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPaEstimated from similar Al alloys.
Shear Strength 285 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000570 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.864 J/g-°C
Thermal Conductivity 120 W/m-K
Melting Point 1010 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 1010 °FAA; Typical
Liquidus 1190 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 995 °F
Aging Temperature 325 - 375 °Ffrom 18 to 36 hr at temperature
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 91.5 - 93.8 %As remainder
Copper, Cu 5.8 - 6.8 %
Iron, Fe <= 0.30 %
Magnesium, Mg <= 0.02 %
Manganese, Mn 0.20 - 0.40 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.20 %
Titanium, Ti 0.02 - 0.10 %
Vanadium, V 0.05 - 0.15 %
Zinc, Zn <= 0.10 %
Zirconium, Zr 0.10 - 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2219-T81
Aluminum 2219-T62
Aluminum 2219-T851
Aluminum 2014-T6; 2014-T651
302 Stainless Steel, 60% cold reduction

MA2219T851a / 170633

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.