MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Polycasa CAST PMMA
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, Cast

Material Notes: QUINN CAST has an optical transparency of 93% light transmission for transparent sheets. It is significantly lighter and much more impact resistant than glass of equivalent thickness. QUINN CAST is resistant to UV rays, shows good thermal stability and low water absorption. QUINN CAST sheets are easy to handle and most fabricating and molding techniques are applicable to it, allowing attractive designs.

Construction

  • Skylights
  • Barrel Vaults
  • Partitions
  • Doors

Industry

  • Signs
  • Displays
  • Furniture
  • Sanitary fittings
  • Gift Articles
  • Shop fittings
  • Solariums
  • Boat Windows
  • Projection Screens

Quinn Manufacturing Group rebranded its Plastics Division as Polycasa in 2013.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.19 g/ccISO 1183
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 105ISO 2039-2
Tensile Strength at Break 75.0 MPaISO 527
Elongation at Break 6.0 %ISO 527
Tensile Modulus 3.30 GPaISO 527
Flexural Strength 125 MPaISO 178
Flexural Modulus 3.00 GPaISO 178
Charpy Impact Unnotched 1.50 J/cm²ISO 179
Charpy Impact, Notched 0.200 J/cm²ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmDIN 53482
Surface Resistance 1.00e+14 ohmDIN 53482
Dielectric Constant 3.6
@Frequency 50 Hz
Dielectric Strength 30.0 kV/mmDIN 53481
Dissipation Factor 0.060
@Frequency 50 Hz
DIN 53483
 
Thermal PropertiesOriginal ValueComments
CTE, linear 70.0 µm/m-°C
@Temperature 20.0 °C
ISO 11359-2
Specific Heat Capacity 2.16 J/g-°CISO 3146-C-60ºC
Thermal Conductivity 0.190 W/m-KDIN 52612
Maximum Service Temperature, Air 80.0 °CContinuous Use
 90.0 °CShort Term Use
Deflection Temperature at 1.8 MPa (264 psi) 105 °Cno pressure specified; ISO 75
Vicat Softening Point 115 °CISO 306
Decomposition Temperature >= 280 °C
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.492ISO 489
Transmission, Visible 93 %ISO 1183
 
Processing PropertiesOriginal ValueComments
Processing Temperature 160 - 190 °CSheet Forming

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lucite International Perspex™ GS Acrylic Cast Sheet 000/0000
Overview of materials for Acrylic, Cast
Röhm Acrylite® GP Acrylic Sheet, Cast
Spartech Polycast Solarcryl (0.187") Cell Cast Acrylic
Carpenter Thermo-Span® Fe-Co-Ni Superalloy

PSF0232 / 66583

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.