MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes Multimet® alloy, investment-cast, as-cast
Categories: Metal; Superalloy; Iron Base

Material Notes: Recommended for use in applications involving high stress at temperatures up to 816°C (1500°F), and moderate stresses up to 1093°C (2000°F). Excellent oxidation resistance, good ductility, and is readily fabricated. Current applications include aircraft, including tailpipes and tailcones, afterburner parts, exhaust manifolds, combustion chambers, turbine blades, buckets and nozzles. Excellent service for high temperature bolts.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: AMS 5794, UNS R30155, AMS 5532, AMS 5768, AMS 5769, AMS 5795
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.20 g/cc0.296 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 241241Converted from Rockwell C hardness.
Hardness, Knoop 255255Converted from Rockwell C hardness.
Hardness, Rockwell C 2121
Hardness, Vickers 247247Converted from Rockwell C hardness.
Tensile Strength, Ultimate 676 MPa98000 psi
Tensile Strength, Yield 399 MPa
@Strain 0.2 %
57900 psi
@Strain 0.2 %
Elongation at Break 27 %27 %in 25.4 mm
Reduction of Area 24 %24 %
Poissons Ratio 0.2980.298RT
 0.315
@Temperature 426 °C
0.315
@Temperature 799 °F
 0.319
@Temperature -78.0 °C
0.319
@Temperature -108 °F
 0.325
@Temperature 650 °C
0.325
@Temperature 1200 °F
 0.339
@Temperature 816 °C
0.339
@Temperature 1500 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000930 ohm-cm
@Temperature 22.0 °C
0.0000930 ohm-cm
@Temperature 71.6 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  15.3 µm/m-°C
@Temperature 23.0 - 300 °C
8.50 µin/in-°F
@Temperature 73.4 - 572 °F
 15.6 µm/m-°C
@Temperature 23.0 - 400 °C
8.67 µin/in-°F
@Temperature 73.4 - 752 °F
 16.0 µm/m-°C
@Temperature 23.0 - 500 °C
8.89 µin/in-°F
@Temperature 73.4 - 932 °F
 16.7 µm/m-°C
@Temperature 23.0 - 600 °C
9.28 µin/in-°F
@Temperature 73.4 - 1110 °F
 17.2 µm/m-°C
@Temperature 23.0 - 700 °C
9.56 µin/in-°F
@Temperature 73.4 - 1290 °F
 17.5 µm/m-°C
@Temperature 23.0 - 800 °C
9.72 µin/in-°F
@Temperature 73.4 - 1470 °F
 17.8 µm/m-°C
@Temperature 23.0 - 900 °C
9.89 µin/in-°F
@Temperature 73.4 - 1650 °F
 17.8 µm/m-°C
@Temperature 23.0 - 1000 °C
9.89 µin/in-°F
@Temperature 73.4 - 1830 °F
 18.4 µm/m-°C
@Temperature 23.0 - 1100 °C
10.2 µin/in-°F
@Temperature 73.4 - 2010 °F
Specific Heat Capacity 0.435 J/g-°C
@Temperature >=100 °C
0.104 BTU/lb-°F
@Temperature >=212 °F
Thermal Conductivity  15.9 W/m-K
@Temperature 300 °C
110 BTU-in/hr-ft²-°F
@Temperature 572 °F
 17.3 W/m-K
@Temperature 400 °C
120 BTU-in/hr-ft²-°F
@Temperature 752 °F
 18.6 W/m-K
@Temperature 500 °C
129 BTU-in/hr-ft²-°F
@Temperature 932 °F
 20.0 W/m-K
@Temperature 600 °C
139 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 20.0 W/m-K
@Temperature 200 °C
139 BTU-in/hr-ft²-°F
@Temperature 392 °F
Melting Point 1288 - 1354 °C2350 - 2469 °F
Solidus 1288 °C2350 °F
Liquidus 1354 °C2469 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.88
@Temperature 1090 °C
0.88
@Temperature 1990 °F
Oxidized
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.080 - 0.16 %0.080 - 0.16 %
Cb + Ta 0.75 - 1.25 %0.75 - 1.25 %
Chromium, Cr 20 - 22.5 %20 - 22.5 %
Cobalt, Co 18.5 - 21 %18.5 - 21 %
Iron, Fe 33 %33 %As remainder
Manganese, Mn 1.0 - 2.0 %1.0 - 2.0 %
Molybdenum, Mo 2.5 - 3.5 %2.5 - 3.5 %
Nickel, Ni 19 - 21 %19 - 21 %
Nitrogen, N 0.10 - 0.20 %0.10 - 0.20 %
Silicon, Si <= 1.0 %<= 1.0 %
Tungsten, W 2.0 - 3.0 %2.0 - 3.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allvac® Nickelvac® 625 Nickel Superalloy, Heat Treatment: 927°C (1700°F) Anneal
Haynes 188 alloy, cold rolled and 1175°C solution annealed sheet
446 Stainless Steel, Annealed Strip
CoorsTek ACI-Ni10 Tungsten Carbide
ATI Allvac® Nickelvac® H-X Nickel Superalloy, Heat Treatment: 1177°C (2150°F) Anneal

NHAMBS / 16835

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.