MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 5086-H112
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: This alloy has very good corrosion resistance (susceptible to deterioration after prolonged exposure to elevated temperatures) and moderate strength. Its weldability is a plus. It is used similarly to aluminum 5083 (although 5086 has better stress corrosion cracking resistance) - in transportation, pressure vessels, cryogenics, towers and drilling rigs, gas/oil piping, ordnance, and armor plate.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A95086; ISO AlMg4; Aluminium 5086-H112; AA5086-H112; Al5086-H112
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.66 g/cc0.0961 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 7373500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 9696Converted from Brinell Hardness Value
Hardness, Vickers 8383Converted from Brinell Hardness Value
Tensile Strength, Ultimate 269 MPa39000 psiAA; Typical
 >= 235 MPa
@Thickness 50.83 - 76.2 mm
>= 34100 psi
@Thickness 2.001 - 3.00 in
 >= 240 MPa
@Thickness 12.7 - 25.4 mm
>= 34800 psi
@Thickness 0.500 - 1.00 in
 >= 240 MPa
@Thickness 25.43 - 50.8 mm
>= 34800 psi
@Thickness 1.001 - 2.00 in
 >= 250 MPa
@Thickness 4.78 - 12.7 mm
>= 36300 psi
@Thickness 0.188 - 0.499 in
Tensile Strength, Yield 131 MPa19000 psiAA; Typical
 >= 95.0 MPa
@Thickness 25.43 - 50.8 mm
>= 13800 psi
@Thickness 1.001 - 2.00 in
 >= 95.0 MPa
@Thickness 50.83 - 76.2 mm
>= 13800 psi
@Thickness 2.001 - 3.00 in
 >= 110 MPa
@Thickness 12.7 - 25.4 mm
>= 16000 psi
@Thickness 0.500 - 1.00 in
 >= 125 MPa
@Thickness 4.78 - 12.7 mm
>= 18100 psi
@Thickness 0.188 - 0.499 in
Elongation at Break  >= 8.0 %
@Thickness 4.78 - 12.7 mm
>= 8.0 %
@Thickness 0.188 - 0.499 in
 >= 10 %
@Thickness 12.7 - 25.4 mm
>= 10 %
@Thickness 0.500 - 1.00 in
 >= 14 %
@Thickness 25.43 - 50.8 mm
>= 14 %
@Thickness 1.001 - 2.00 in
 >= 14 %
@Thickness 50.83 - 76.2 mm
>= 14 %
@Thickness 2.001 - 3.00 in
 14 %
@Thickness 1.59 mm
14 %
@Thickness 0.0625 in
AA; Typical
Modulus of Elasticity 71.0 GPa10300 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Tensile Modulus 71.0 GPa10300 ksi
Compressive Strength 270 MPa39200 psi
Compressive Modulus 72.4 GPa10500 ksi
Poissons Ratio 0.330.33
Shear Modulus 26.4 GPa3830 ksi
Shear Strength 160 MPa23200 psiCalculated value.
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000549 ohm-cm
@Temperature 20.0 °C
0.00000549 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  22.0 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.2 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.8 µm/m-°C
@Temperature 20.0 - 100 °C
13.2 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 24.7 µm/m-°C
@Temperature 20.0 - 200 °C
13.7 µin/in-°F
@Temperature 68.0 - 392 °F
 25.8 µm/m-°C
@Temperature 20.0 - 300 °C
14.3 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.900 J/g-°C0.215 BTU/lb-°F
Thermal Conductivity 125 W/m-K870 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 585.0 - 640.6 °C1085 - 1185 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 585.0 °C1085 °FAA; Typical
Liquidus 640.6 °C1185 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 343 °C650 °Fholding at temperature not required
Hot-Working Temperature 316 - 482 °C600 - 900 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 93 - 96.3 %93 - 96.3 %As remainder
Chromium, Cr 0.05 - 0.25 %0.05 - 0.25 %
Copper, Cu <= 0.10 %<= 0.10 %
Iron, Fe <= 0.50 %<= 0.50 %
Magnesium, Mg 3.5 - 4.5 %3.5 - 4.5 %
Manganese, Mn 0.20 - 0.70 %0.20 - 0.70 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.40 %<= 0.40 %
Titanium, Ti <= 0.15 %<= 0.15 %
Zinc, Zn <= 0.25 %<= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 5086-O
Alclad Aluminum 6061-T6, T651
6060 Aluminum Composition Spec
Aluminum 5086-H116; 5086-H32
Aluminum 5086-H34

MA5086H112 / 9187

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.