MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
BASF Ultramid® 8270 HS BK 102 PA6 (Dry)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: Description: Ultramid 8270 HS BK-102 is a thermally modified pigmented black, PA6 blow molding compound exhibiting exceptional toughness and melt strength ideally suited for blow molding, profile extrusion, and other applications requiring extra high melt viscosity. It exhibits excellent permeability and chemical resistance to oils, hydrocarbons and most solvents.

Applications: Industrial containers, small gasoline tanks, and automotive under hood reservoirs.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.13 g/ccASTM D792
Moisture Absorption at Equilibrium 1.6 %24 Hours; ASTM D570
 2.6 %50% RH; ASTM D570
 9.2 %Saturation; ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 99ASTM D785
Tensile Strength, Yield 24.0 MPa
@Temperature 121 °C
ASTM D638
 84.0 MPa
@Temperature 23.0 °C
ASTM D638
 138 MPa
@Temperature -40.0 °C
ASTM D638
Elongation at Break >= 100 %ASTM D638
Elongation at Yield 4.0 %ASTM D638
Flexural Strength 17.0 MPa
@Temperature 121 °C
ASTM D790
 20.0 MPa
@Temperature 90.0 °C
ASTM D790
 30.0 MPa
@Temperature 65.0 °C
ASTM D790
 114 MPa
@Temperature 23.0 °C
ASTM D790
 179 MPa
@Temperature -40.0 °C
ASTM D790
Flexural Modulus 260 MPa
@Temperature 121 °C
ASTM D790
 310 MPa
@Temperature 90.0 °C
ASTM D790
 435 MPa
@Temperature 65.0 °C
ASTM D790
 2900 MPa
@Temperature 23.0 °C
ASTM D790
 3160 MPa
@Temperature -40.0 °C
ASTM D790
Izod Impact, Notched 53.0 J/m
@Temperature -40.0 °C
ASTM D256
 53.0 J/m
@Temperature 23.0 °C
ASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear 135 µm/m-°CASTM E831
Melting Point 220 °CASTM D3418
Deflection Temperature at 0.46 MPa (66 psi) 169 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 63.0 °CASTM D648
 
Processing PropertiesOriginal ValueComments
Melt Temperature 245 - 260 °C
Mold Temperature 60.0 °C
Dry Time 2 - 4 hour
Moisture Content <= 0.15 %
 
Descriptive Properties
ColorBK 102
Commercial StatusNorth America

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® 8270 HS PA6 (Dry)
BASF Ultramid® 8270 HS BK 102 PA6 (Conditioned)
Nylene® NX4301 Nylon 6, Extrusion Grade
BASF Ultramid® 8270 HS PA6 (Conditioned)
BASF Ultramid® 8254 HS BK-102 PA6 (Dry)

PBASG0449 / 132082

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.