MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Naval Brass, Uninhibited, Copper Alloy, UNS C46400 , H01 Temper, Flat Products
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass

Material Notes: Temper: 1/4 Hard

Excellent Suitability – Soldering, Brazing, Capacity for Being Hot Formed; Good Suitability – Oxyacetylene Welding, Spot Weld, Butt Weld; Fair Suitability – Gas Shielded Arc Welding, Seam Weld, Capacity for Being Cold Worked

Common Fabrication Processes: Blanking; Drawing; Forming and Bending; Heading and Upsetting; Hot Forging and Pressing; hot heading and upsetting; Shearing

Typical Uses: Lock Pins; Precision Shipboard Equipment; Bolts; Nuts; Rivets; Aircraft Turn buckle Barrels; Balls; Bearings; Condenser Plates; Dies, Golf Ball Production; Heat Exchanger Tube; Hub Cones; Pressure Vessels; Structural Uses; Valve Stems; Welding Rod; Decorative Fittings; Marine Hardware; Propeller Shafts; Shafting; Turn buckles; Missile Components; Baffle Plates and Flanges; Fittings

Applicable Specifications: Bar – SAE J461, SAE J463, AMS 4612, Forgings ASTM B124/B124M, AMS 4611, FEDERAL Q-B-639, ASTM B21/B21M; Bolts – ASTM F468; Forgings, Die (Hot Pressed) – ASTM B283/B283M, ASME SB283; Nuts – ASTM F467; Plate – FEDERAL QQ-B-639, ASTM B432; Plate & Sheet - for Pressure Vessels, Condensers & Heat Exchangers ASME SB171, for Pressure Vessels, Condensers & Heat Exchangers ASTM B171/B171M; Rod – AMS 4612, ASTM B21/B21M, SAE J463, SAE J461, AMS 4611, Forgings ASTM B124/B124M; Screws – ASTM F468; Shapes – Forgings ASTM B124/B124M, ASTM B21/B21M; Sheet – FEDERAL QQ-B-639; Strip – SAE J463, FEDERAL QQ-B-639, SAE J461; Studs – ASTM F468; Wire – MILITARY MIL-W-6712

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.304 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 75
@Thickness 1.02 mm
Hardness, Rockwell 30T 68
@Thickness 1.02 mm
Tensile Strength 70.0 ksi
@Thickness 1.02 mm
Elongation at Break 17 %
@Thickness 1.02 mm
Tensile Modulus 15000 ksi
Modulus of Rigidity 5600 ksi
Poissons Ratio 0.34Calculated
Machinability 30 %
Forgeability 90 %
Shear Strength 43.0 ksi
@Thickness 1.02 mm
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000610 ohm-cm28% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.8 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0900 BTU/lb-°F
Thermal Conductivity 67.0 BTU-in/hr-ft²-°F
Melting Point 1630 - 1650 °F
Solidus 1630 °F
Liquidus 1650 °F
Annealing Point 800 - 1100 °F
 
Processing PropertiesOriginal ValueComments
Hot-Working Temperature 1200 - 1500 °F
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 59 - 62 %
Iron, Fe <= 0.10 %
Lead, Pb <= 0.20 %
Tin, Sn 0.50 - 1.0 %
Zinc, Zn 36.8 - 40.5 %As Balance

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC46400x1 / 292026

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.