MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LyondellBasell Astryn 68F4-2 Polypropylene Homopolymer, 20% Talc  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes:
Key Features: fractional melt flow, medium high modulus, mineral-filled, blow molding and extrusion grade polypropylene homopolymer, excellent impact and stiffness balance, good processability

Applications: automotive under-the-hood components

Description: Astryn 68F4-2 fraction melt flow, 20% talc-filled, blow molding and extrusion grade polypropylene homopolymer is designed for high strength, stiffness, impact resistance and processability.

Information provided by Montell Polyolefins.

LyondellBasell is the successor company to Montell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccASTM D792B
Melt Flow 0.60 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 96ASTM D785
Tensile Strength, Ultimate 26.0 MPaASTM D638
Tensile Strength, Yield 34.0 MPaASTM D638
Elongation at Break 160 %ASTM D638
Elongation at Yield 8.0 %ASTM D638
Flexural Modulus 1.70 GPaTangent at 0.05 in/min; ASTM D790A
Izod Impact, Notched 1.10 J/cmASTM D256A
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 100 °CASTM D648

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LyondellBasell Moplen HP550J Polypropylene Homopolymer
LyondellBasell Hostacom™ GP622 Polypropylene Homopolymer
LyondellBasell Astryn 65F4-2 Polypropylene Homopolymer, 20% Talc
LyondellBasell Astryn 65F4-3 Polypropylene Homopolymer, 30% Talc
Niche Polymer PPHT40BK Homopolymer PP, 40% Talc Fiber Filled

PMO345 / 53604

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.