MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ExxonMobil Santoprene® 261-87 Thermoplastic Elastomer  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: A hard, colorable thermoplastic vulcanizate (TPV) in the thermoplastic elastomer (TPE) family. This material has good fluid resistance for use in wet electrical wire and cable applications. This grade of Santoprene TPV is shear-dependent and can be processed on conventional thermoplastics equipment for injection molding, extrusion or blow molding. It is polyolefin based and completely recyclable.

Polymeric Materials for Use in Wire and Cable

Information provided by Advanced Elastomer Systems

Key Words: EU 2003/11/EC; RoHS Compliant; UL QMFZ2; UL QMFZ8
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.970 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 87.12 in; ASTM D2240
Tensile Strength at Break 2300 psiAcross Flow; ASTM D412
Tensile Strength, Ultimate 970 psiAcross Flow; ASTM D412
Elongation at Break 640 %Across Flow; ASTM D412
 
Processing PropertiesOriginal ValueComments
Processing Temperature 175 - 230 °C
Mold Temperature 50.0 - 125 °FProcessing
Drying Temperature 180 °F
Dry Time 3 hour
Moisture Content 0.080 %
Back Pressure 50.0 - 100 psiProcessing
Clamp Pressure 6000 - 10000 psi
Vent Depth 0.00100 in
Cushion 0.125 - 0.250 in
Screw Speed 100 - 200 rpm
 
Descriptive Properties
ColorNatural Color
FormPellets
Injection RateFast
Maximum Regrind %20
Screw Compression Ratio2:1 - 2.5:1
Screw L/D Ratio16:1 - 20:1

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Alliance Polymers Viprene™ P80A-22U-BLK Thermoplastic Vulcanizate Elastomer
Buckeye Polymers BP FLEX A 0505 Soft Touch TPE
ExxonMobil Santoprene® 171-73 Thermoplastic Elastomer
ExxonMobil Santoprene® 221-87 Thermoplastic Elastomer
Alliance Polymers Viprene™ G90A-32U-NAT Thermoplastic Vulcanizate Elastomer

PADVA127 / 22817

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.