MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ExxonMobil Santoprene® 521-70 Thermoplastic Rubber  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Elastomer, Melt-Processible Rubber

Material Notes: A black thermoplastic elastomer designed for glazing and sealing applications with good fluid resistance, formulated to replace thermoset elastomers such as EPDM, polychloroprene, and chlorosulfonated polyethylene. It can be processed using injection molding, extrusion, blow molding or other melt processing techniques.

Key Features: Recommended for glazing and sealing applications; Good UV stability; Passes ASTM C 542 Flame Test requirement; Good low temperature flexibility

Additional processing comments: This thermoplastic rubber is a shear-dependent material that can be processed on conventional thermoplastic equipment for injection molding, extrusion, or blow molding. For extrusion, a general purpose screw with a compression ratio of 2.5 to 3.0 is recommended. Material can be recycled. SANTOPRENE rubber is incompatible with acetal and PVC.

Values below are for injection molded plaques, side gated, 82.6 mm x 117.5 mm x 3.0 mm. Tensile properties measured across flow. Data provided by Advanced Elastomer Systems.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.08 g/ccTPE-0105 (ASTM D792)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 705 Second; TPE-0169 (ASTM D 2240)
Tensile Strength, Ultimate 6.70 MPaTPE-0153 (ASTM D 412)
Elongation at Break 460 %TPE-0153 (ASTM D 412)
100% Modulus 0.00380 GPa
@Strain 100 %
TPE-0153 (ASTM D 412)
Graves Tear Strength 25.0 kN/mTPE-0056 (ASTM D 624)
Compression Set 37 %
@Temperature 100 °C
168 hrs.; TPE-0016 (ASTM D 412)
Tensile Set 11.5 %TPE-0053 (ASTM D 412)
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature <= -57.0 °CTPE-0089 (ASTM D 746)
 
Processing PropertiesOriginal ValueComments
Processing Temperature 177 - 232 °C
Drying Temperature 82.0 °CDesiccant drying for 3 hours recommended
Dry Time 3 hour

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ExxonMobil Santoprene® 121-80M300 Thermoplastic Rubber
ExxonMobil Santoprene® 8211-45W237 Thermoplastic Rubber
ExxonMobil Santoprene® 121-70B230 Thermoplastic Elastomer
ExxonMobil Vyram™ 9201-75 Thermoplastic Elastomer
ExxonMobil Santoprene® 121-65W233 Thermoplastic Elastomer

PADW00 / 22852

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.