Noble Polymers Ecobarrier™ 0918 Thermoplastic Olefin (TPO)
Categories:
Polymer
;
Thermoplastic
;
Elastomer, TPE
;
Olefinic TPE
;
Thermoplastic Olefinic Elastomer (TPO)
;
TPO
Material Notes:
Ecobarrier is a TPO (thermoplastic olefin) produced by Noble Polymers based on olefin/elastomer compounding. Ecobarrier is primarily used as a sound barrier material in low heat applications.
Information provided by Noble Polymers.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.82
g/cc
1.82
g/cc
ASTM D792
Melt Flow
19.35
g/10 min
@Load 2.16 kg,
Temperature 230 °C
19.35
g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Hardness, Shore A
80
80
ASTM D2240
Tensile Strength at Break
2.95
MPa
428
psi
ASTM D412
Elongation at Break
132 %
132 %
ASTM D412
2% Secant Modulus
0.05904
GPa
8.563
ksi
ASTM D790
Tear Strength
42.72
kN/m
243.7
pli
ASTM D624
Processing Properties
Metric
English
Comments
Middle Barrel Temperature
191
-
218
°C
375
-
425
°F
Ejection Temperature
26.7
-
54.4
°C
80.0
-
130
°F
Water Temperature
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Noble Polymers Ecobarrier™ 0414 Thermoplastic Olefin (TPO)
Noble Polymers Ecobarrier™ 0512 Thermoplastic Olefin (TPO)
A. Schulman INVISION™ VX-5170UE Soft Touch Polyolefin Thermoplastic
Avient Elastamax™ XL-2065 Thermoplastic Polyolefin Elastomer (TPO (POE))
Noble Polymers Ecobarrier™ 1512 Thermoplastic Olefin (TPO)
PNOBLE09 / 54819
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.