MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Nylon 66, Aramid Fiber Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Aramid Fiber Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, Aramid Fiber Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.14 - 1.32 g/ccAverage value: 1.21 g/cc Grade Count:45
Filler Content 5.00 - 20.0 %Average value: 13.6 % Grade Count:7
Water Absorption 0.500 - 1.00 %Average value: 0.834 % Grade Count:16
Additive Loading 10.0 - 15.0 %Average value: 11.4 % Grade Count:7
Linear Mold Shrinkage 0.00100 - 0.0300 cm/cmAverage value: 0.0121 cm/cm Grade Count:40
Linear Mold Shrinkage, Transverse 0.00500 - 0.0240 cm/cmAverage value: 0.0171 cm/cm Grade Count:8
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 100 - 120Average value: 113 Grade Count:8
Tensile Strength, Ultimate 48.3 - 138 MPaAverage value: 88.1 MPa Grade Count:40
Tensile Strength, Yield 81.4 - 110 MPaAverage value: 92.5 MPa Grade Count:8
 35.0 - 45.0 MPa
@Temperature 90.0 - 120 °C
Average value: 40.0 MPa Grade Count:1
Elongation at Break 1.60 - 10.0 %Average value: 5.26 % Grade Count:46
Modulus of Elasticity 2.41 - 11.0 GPaAverage value: 5.02 GPa Grade Count:37
 0.850 - 1.20 GPa
@Temperature 90.0 - 120 °C
Average value: 1.03 GPa Grade Count:1
Flexural Yield Strength 75.8 - 207 MPaAverage value: 132 MPa Grade Count:44
Flexural Modulus 0.621 - 8.69 GPaAverage value: 4.08 GPa Grade Count:44
Izod Impact, Notched 0.320 - 1.44 J/cmAverage value: 0.595 J/cm Grade Count:36
Izod Impact, Unnotched 2.14 - 11.2 J/cmAverage value: 5.43 J/cm Grade Count:28
Izod Impact, Notched (ISO) 4.00 - 5.80 kJ/m²Average value: 4.86 kJ/m² Grade Count:5
Izod Impact, Unnotched (ISO) 37.0 - 48.6 kJ/m²Average value: 40.7 kJ/m² Grade Count:4
Charpy Impact Unnotched 1.50 - 5.00 J/cm²Average value: 2.93 J/cm² Grade Count:6
Charpy Impact, Notched 0.150 - 1.50 J/cm²Average value: 0.675 J/cm² Grade Count:10
Coefficient of Friction 0.130 - 0.550Average value: 0.312 Grade Count:6
Coefficient of Friction, Static 0.130 - 0.460Average value: 0.290 Grade Count:6
K (wear) Factor 7.50 - 46.3 x 10-8 mm³/N-MAverage value: 25.4 x 10-8 mm³/N-M Grade Count:6
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1e+05 - 1.00e+17 ohm-cmAverage value: 5.92e+15 ohm-cm Grade Count:23
Surface Resistance 1.00e+13 - 1.00e+14 ohmAverage value: 5.50e+13 ohm Grade Count:4
Dielectric Strength 17.7 - 30.0 kV/mmAverage value: 20.6 kV/mm Grade Count:5
 
Thermal PropertiesOriginal ValueComments
CTE, linear 27.0 - 81.0 µm/m-°CAverage value: 54.9 µm/m-°C Grade Count:12
CTE, linear, Transverse to Flow 91.8 - 97.0 µm/m-°CAverage value: 95.3 µm/m-°C Grade Count:3
Thermal Conductivity 0.230 - 0.346 W/m-KAverage value: 0.302 W/m-K Grade Count:3
Melting Point 255 - 265 °CAverage value: 259 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 232 - 251 °CAverage value: 240 °C Grade Count:18
Deflection Temperature at 1.8 MPa (264 psi) 85.0 - 246 °CAverage value: 164 °C Grade Count:39
Vicat Softening Point 245 - 260 °CAverage value: 248 °C Grade Count:5
Flammability, UL94 HBGrade Count:25
 
Processing PropertiesOriginal ValueComments
Processing Temperature 70.0 - 300 °CAverage value: 237 °C Grade Count:13
Nozzle Temperature 280 - 315 °CAverage value: 302 °C Grade Count:3
Melt Temperature 260 - 315 °CAverage value: 290 °C Grade Count:30
Mold Temperature 60.0 - 120 °CAverage value: 87.3 °C Grade Count:38
Drying Temperature 70.0 - 105 °CAverage value: 81.6 °C Grade Count:30
Moisture Content 0.100 - 0.200 %Average value: 0.195 % Grade Count:23
Dew Point -17.8 °CAverage value: -17.8 °C Grade Count:14
Injection Pressure 30.0 - 124 MPaAverage value: 98.0 MPa Grade Count:24

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Acetal Copolymer, Aramid Fiber Filled
DuPont™ Kevlar® 49 Aramid Fiber
Overview of materials for Polyetheretherketone, PEEK, Aramid Fiber Filled
Eurotec® Tecomid® NA40 AR20 NL HS PA6.6, 20% aramid fiber reinforced, heat stabilized, natural
Overview of materials for Nylon 6, Unreinforced

O2527 / 78025

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.