MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Bohler-Uddeholm P20 PREMIUM MODIFIED Pre-hardened Mold Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Chrome-moly Steel; Tool Steel; Mold Steel

Material Notes: Cr-Mo alloyed steel

P20 Modified offers the following benefits:

  • No hardening risks
  • No hardening costs
  • Time saving, e.g. no waiting for heat treatment
  • Lower tool cost (e.g. no distortion to rectify)
  • Modifications easily carried out
  • Can be subsequently nitrided to increase surface wear resistance or locally flame hardened to reduce surface damage.
      Manufactured to consistently high quality standards, P20 modified has good polishing and texturing properties, good machinability and uniformed hardness.
      Heavier sections are supplied premachined which offers the following advantages compared with unmachined material:
      • Saving of weight
      • Non-decarburized surface
      • Exact nominal size (plus tolerance)
      • Less machining
      • Absence of scale minimizes machine and tool wear
      Applications:
      • For large injection and compression molds
      • Extrusion dies for thermoplastics
      • Blow mold
      • High strength holders, plates and bolsters
      • Forming tools, press-brake dies (possibly flame hardened or nitrided)
      • Aluminum die casting prototype dies
      • Zinc die casting dies
      • Long run die shoes
      • Structural components, shafts.

Key Words: AISI P20 modified
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.282 lb/in³hardened to 310 HB
 0.280 lb/in³
@Temperature 199 °C
hardened to 310 HB
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 285 - 340Hardened and tempered (Delivery condition)
Tensile Strength, Ultimate 138000 - 160000 psihardened to 300 HB
Tensile Strength, Yield >= 101000 psihardened to 300 HB
Elongation at Break >= 12 %hardened to 300 HB
Modulus of Elasticity 29700 ksi(hardened to 310 HB)
 29000 ksi
@Temperature 199 °C
hardened to 310 HB
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.00 µin/in-°F
@Temperature 199 °C
hardened to 310 HB
Specific Heat Capacity 0.110 BTU/lb-°F
@Temperature 20.0 °C
hardened to 310 HB
Thermal Conductivity 29.0 W/m-K
@Temperature 20.0 °C
hardened to 310 HB
 29.5 W/m-K
@Temperature 199 °C
hardened to 310 HB

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type P20 Mold Steel (UNS T51620)
Schmolz + Bickenbach P-20 High Hard Plastic Mold Steel
EDRO #3 Prehardened Mold Quality P20 Alloy Steel
Schmolz + Bickenbach P-20 Modified Plastic Mold Steel
Bohler-Uddeholm IMPAX® P20 Hot Work Tool Steel

NBUCOR35 / 15504

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.