MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
BASF Ultraform® N 2320 003 AT BK120 POM
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: Ultraform N 2320 003 AT BK120 is a pigmented black, rapidly freezing general-purpose injection molding POM grade. It contains a mold release agent.

Applications: Typical applications include spring elements, clips, gas filler caps, gears wheels, small motor parts, curtain hooks and release buttons for safety belts

Information provided by BASF.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.41 g/ccISO 1183
Moisture Absorption 0.250 %50% RH; ISO 62
Water Absorption at Saturation 0.90 %ISO 62
Linear Mold Shrinkage, Flow 0.021 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.021 cm/cmISO 294-4
Melt Flow 7.5 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 64.0 MPaISO 527
Elongation at Break 25 %ISO 527
Elongation at Yield 10 %ISO 527
Tensile Modulus 2700 MPaISO 527
Izod Impact, Notched (ISO) 5.50 kJ/m²
@Temperature -40.0 °C
ISO 180
 6.00 kJ/m²
@Temperature 23.0 °C
ISO 180
Charpy Impact Unnotched 190 kJ/m²
@Temperature -30.0 °C
ISO 179
 200 kJ/m²
@Temperature 23.0 °C
ISO 179
Charpy Impact, Notched 6.00 kJ/m²
@Temperature -30.0 °C
ISO 179
 6.50 kJ/m²
@Temperature 23.0 °C
ISO 179
Tensile Creep Modulus, 1000 hours 1400 MPaISO 899
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohmIEC 60093
Dielectric Constant 3.8
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.0050
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 110 µm/m-°C
Melting Point 166 °CISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 95.0 °CISO 75
UL RTI, Electrical 105 °C
@Thickness 0.750 mm
UL746B
 105 °C
@Thickness 1.50 mm
UL746B
 105 °C
@Thickness 3.00 mm
UL746B
UL RTI, Mechanical with Impact 90.0 °C
@Thickness 1.50 mm
UL746B
 90.0 °C
@Thickness 3.00 mm
UL746B
UL RTI, Mechanical without Impact 90.0 °C
@Thickness 1.50 mm
UL746B
 105 °C
@Thickness 3.00 mm
UL746B
Flammability, UL94 HB
@Thickness 0.750 mm
 HB
@Thickness 1.50 mm
 HB
@Thickness 3.00 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 190 - 230 °C
Mold Temperature 45.0 - 105 °Ccan be used where applicable
 80.0 - 90.0 °Crecommended
 60.0 - 120 °C
Drying Temperature 80.0 - 110 °C
@Time 7200 - 14400 sec
Moisture Content <= 0.15 %
Injection Pressure 500 - 1000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBASF8922 / 254880

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.