MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Phillips Sumika Marlex® ABF-300 High Flow Thermoplastic Olefin  (discontinued **)
Categories: Polymer; Thermoplastic; Polyolefin

Material Notes: Applications:
  • Automotive exterior fascias

Information provided by Chevron Phillips.

Phillips Sumika Polypropylene Company has been shut down, as announced in 2011.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.890 g/cc
@Thickness 3.17 mm
injection molded specimen; ISO 1133
Melt Flow 30 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 56ISO 868
Tensile Strength, Yield 20.0 MPa50 mm/min, 1/8" thick injection molded specimen; ISO 1183
Flexural Modulus 0.965 GPa
@Thickness 3.17 mm
injection molded specimen, 2 mm/min; ISO 178
Izod Impact, Notched (ISO) 4.50 kJ/m²
@Thickness 3.17 mm,
Temperature -40.0 °C
ISO 180
 45.0 kJ/m²
@Thickness 3.17 mm,
Temperature 23.0 °C
ISO 180
Impact Test 21.0 J
@Temperature 23.0 °C
Instrumented, 2.2 m/s, ductile; ASTM 3763
 29.0 J
@Temperature -30.0 °C
Instrumented, 2.2 m/s, ductile; ASTM D3763
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 79.0 °C
@Thickness 3.17 mm
injection molded specimen; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 48.0 °C
@Thickness 3.17 mm
injection molded specimen; ISO 75

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LyondellBasell Hifax TYC 1235X BLACK Thermoplastic Olefinic Elastomer, mineral Filled
LyondellBasell Hifax TYC 1235X E BLACK Polypropylene, Talc Filled
Noble Polymers Regis™ 235107 Thermoplastic Olefin (TPO)
Overview of materials for Polypropylene with 40% Glass Fiber Filler
Chevron Phillips Marlex® 9398 HDPE Pipe and Corrugated Extrusion Resin

PCHEVD084 / 20668

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.