MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
High-Leaded Tin Bronze, UNS C93500, Copper Casting Alloy
Categories: Metal; Nonferrous Metal; Copper Alloy; Copper Casting Alloy

Material Notes: Casting methods recommended for this alloy: Centrifugal, Continuous, and Sand.

Applications: Small bearings and bushings, bronze backing for babbitt-lined automotive bearings.

Classified under: High-leaded tin bronzes. ASTM B584; formerly ASTM B144-3C

Typical data for sand-cast test bars. Alloy does not respond to heat treating

Key Words: High lead tin bronze, ASTM B584, ASTM B144-3C
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.87 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 60
Tensile Strength, Ultimate 220 MPa
Tensile Strength, Yield 110 MPa
@Strain 0.5 %
Elongation at Break 20 %in 50 mm
Modulus of Elasticity 100 GPa
Compressive Strength 90.0 MPaat permanent set of 0.1%
Machinability 70 %UNS C36000 (free-cutting brass) = 100%
Izod Impact 11.0 J
Charpy Impact 11.0 JV-notch
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000011494 ohm-cm
@Temperature 20.0 °C
Magnetic Permeability 1.0
 
Thermal PropertiesOriginal ValueComments
CTE, linear 18.0 µm/m-°C
@Temperature 20.0 - 200 °C
Specific Heat Capacity 0.376 J/g-°C
Thermal Conductivity 71.0 W/m-K
@Temperature 20.0 °C
Melting Point 315 °CIncipient
 855 - 1000 °C
Solidus 855 °C
Liquidus 1000 °C
Shrinkage 1.6 %Patternmaker's Shrinkage (3/16 in./ft.)
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 260 °CStress-Relieving Temperature
 
Component Elements PropertiesOriginal ValueComments
Antimony, Sb <= 0.30 %
Copper, Cu 83 - 86 %
Iron, Fe <= 0.20 %
Lead, Pb 8.0 - 10 %
Nickel, Ni <= 0.50 %
Phosphorus, P <= 0.020 %
Silicon, Si <= 0.0030 %
Sulfur, S <= 0.080 %
Tin, Sn 4.5 - 6.0 %
Zinc, Zn <= 2.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
High-Leaded Tin Bronze, UNS C93900, Copper Casting Alloy
High-Leaded Tin Bronze, UNS C93400, Copper Casting Alloy
High-Leaded Tin Bronze, UNS C93200, Copper Casting Alloy, Bearing Bronze SAE 660
High-Leaded Tin Bronze, UNS C94300, Copper Casting Alloy
High-Leaded Tin Bronze, UNS C93800, Copper Casting Alloy, Sand-Cast

MC93500b1 / 11947

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.