MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Plenco 7021 Black Impact Grade Phenolic Molding Compound
Categories: Polymer; Thermoset; Phenolic; Phenolic, Novolac, Impact Grade, Filled

Material Notes: Plaslok 7021 is the replacement material for the former Union Carbide BMRS-7021. It is a two-stage, impact grade phenolic molding compound suitable for compression, transfer or injection molding of switchgear parts, or where mechanical assembly requires better impact strength.

Data provided by Plaslok Corporation.

Plaslok Corporation was purchased by Plastics Engineering Company in March 2000. The Plaslok name is no longer used on any products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.38 g/ccASTM D792
Apparent Bulk Density 0.480 g/ccASTM D1895
Water Absorption 0.50 %ASTM D570
Linear Mold Shrinkage 0.0060 cm/cmCompression; ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 41.0 MPaASTM D638
Flexural Yield Strength 74.0 MPaASTM D790
Flexural Modulus 6.90 GPaASTM D790
Compressive Yield Strength 228 MPaASTM D695
Izod Impact, Notched 0.240 J/cmASTM D256
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 6.00e+9 ohm-cmASTM D257
Dielectric Constant 4.5
@Frequency 1e+6 Hz
ASTM D150
 6.0
@Frequency 60 Hz
ASTM D150
Dielectric Strength 11.8 kV/mmASTM D149
Dissipation Factor 0.040
@Frequency 1e+6 Hz
ASTM D150
 0.11
@Frequency 60 Hz
ASTM D150
Comparative Tracking Index 125 VUL 746
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 171 °CASTM D648
UL RTI, Electrical 150 °C
@Thickness 1.57 mm
UL RTI, Mechanical with Impact 150 °C
@Thickness 1.57 mm
UL RTI, Mechanical without Impact 150 °C
@Thickness 1.57 mm
Flammability, UL94 V-0
@Thickness 3.18 mm
 V-0
@Thickness 3.18 mm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Kolon KOCETAL® VT702 Anti-Static Grade Acetal Resin
Kolon Kocetal® DP301 Modified Grade Acetal Copolymer
Resinlab® EP950G Gray Aluminum Filled Rubber Modified Epoxy
Quantum PEEK 30% Carbon Filled
Epoxy Technology EPO-TEK® T6067-T Thermally Conductive, Electrically Insulating Epoxy

PLEO918 / 50807

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.