MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LG Chemical KEYFLEX BT 3140D Ester Type TPE  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester, TP; Polyester Thermoplastic Elastomer

Material Notes: Description: Injection Molding, TPC-ET, Specialty, Low Melting Temperature, Low Modulus

Application: Masterbatch Carrier, Cable Compound Base

CAS: 37282-12-5

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.16 g/ccASTM D792
Molecular Weight 458.458 g/mol
Maximum Moisture Content 0.010Injection Molding
 0.010Extrusion Molding
Melt Flow 8.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 90ASTM D2240
Hardness, Shore D 36ASTM D2240
Tensile Strength at Break 29.1 MPa
@Thickness 2.00 mm
50mm/min; ASTM D638
Elongation at Break 700 %
@Thickness 2.00 mm
50mm/min; ASTM D638
Flexural Modulus 550 kg(f)/cm²
@Thickness 6.40 mm
15mm/min; ASTM D790
Izod Impact, Notched NB
@Thickness 6.40 mm,
Temperature 23.0 °C
ASTM D256
 NB
@Thickness 6.40 mm,
Temperature -40.0 °C
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+14 ohm-cmASTM D257
Dielectric Strength 26.0 kV/mm
@Thickness 1.00 mm
ASTM D149
Comparative Tracking Index 600 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 150 °CPeak
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 160 - 180 °CInjection Molding
Middle Barrel Temperature 170 - 190 °CInjection Molding
Front Barrel Temperature 180 - 200 °CInjection Molding
Nozzle Temperature 180 - 200 °CInjection Molding
Zone 1 160 - 180 °CExtrusion Molding
Zone 2 170 - 190 °CExtrusion Molding
Zone 3 180 - 200 °CExtrusion Molding
Zone 4 180 - 200 °CExtrusion Molding
Adapter Temperature 180 - 200 °CExtrusion Molding
Die Temperature 170 - 210 °CExtrusion Molding
Melt Temperature 150 - 200 °CInjection Molding
 150 - 200 °CExtrusion Molding
Mold Temperature 10.0 - 35.0 °CInjection Molding
Drying Temperature 80.0 - 90.0 °CInjection Molding
 80.0 - 90.0 °CExtrusion Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 3.00 - 4.00 hourExtrusion Molding

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LG Chemical KEYFLEX BT 3028D Ester Type TPE
LG Chemical KEYFLEX BT 5035D Ester Type TPE
LG Chemical KEYFLEX BT 3038D Ester Type TPE
LG Chemical KEYFLEX BT 2140D Ester Type TPE
LG Chemical KEYFLEX BT 1030D Ester Type TPE

PLAY440 / 148450

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.