MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

(Viewing data as-entered. Click here to return)
Resinlab® EP1285HD-16 Highly Filled, Medium Viscosity Casting Resin
Categories: Polymer; Thermoset; Epoxy; Epoxy Cure Resin; Epoxy, Cast, Metal Filled

Material Notes: Resinlab™ EP1285 (Formerly Lab Product W021901 series) is a highly filled, medium viscosity black casting resin designed for applications requiring a high degree of thermal conductivity and a low CTE combined with a moderate free flowing viscosity. They give excellent resistance to acids, bases, water, and most organic compounds. The high filler content also enhances resistance to thermal cycle stresses. The choice of hardener allows the user to choose a variety of reactivity’s, viscosities, thermal ranges and environmental resistance capabilities. The resin contains a high loading of abrasive aluminum oxide filler, which can introduce wear considerations for wetted components of meter-mix and dispensing equipment. Warming the assembly prior to filling will aid in flow and air release. Additional vacuum degassing may be desired for some applications.

Information Provided by Resinlab L.L.C., an Ellsworth Adhesives Company.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.12 g/cc
Water Absorption 0.17 %
@Time 86400 sec
TM R050-35
Viscosity 17000 cPMixed, RVT, #6, 2.5 rpm; TM R050-12
Linear Mold Shrinkage 0.0030 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 92TM R050-19
Tensile Strength at Break 4000 psiTM R050-36
Tensile Strength, Ultimate 4000 psiTM R050-36
Tensile Strength, Yield 2000 psiTM R050-36
Elongation at Break 1.0 - 3.0 %TM R050-36
Tensile Modulus 600 ksiTM R050-36
Compressive Yield Strength 6000 psiTM R050-38
Compressive Strength 8000 psiBreak; TM R050-38
 9500 psiUltimate; TM R050-38
Compressive Modulus 500 ksiTM R050-38
Adhesive Bond Strength 2700 psiLap shear; 2024 T3 Al Abraded / MEK Wipe
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cm
Dielectric Constant 5.4
Dielectric Strength 375 V/mil
 
Thermal PropertiesOriginal ValueComments
CTE, linear 39.0 µm/m-°C
@Temperature <=58.0 °C
below Tg
 111 µm/m-°C
@Temperature >=58.0 °C
above Tg
Thermal Conductivity 1.10 W/m-K
Maximum Service Temperature, Air 120 °C
Minimum Service Temperature, Air -60.0 °C
Glass Transition Temp, Tg 58.0 °CTM R050-25
 
Processing PropertiesOriginal ValueComments
Cure Time 2.00 - 4.00 hour
@Temperature 45.0 °C
 8.00 - 16.0 hour
@Temperature 25.0 °C
Pot Life 60 - 90 minMass: 100g; TM R050-17
 
Descriptive Properties
ColorBlack
Mix Ratio13.4:1Weight
 5.7:1Volume

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PRESL124 / 101538

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.