MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AlphaGary Evoprene™ Super G 949 SEBS Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Styrenic TPE

Material Notes: Evoprene™ Super G compounds are high performance styrene ethylene- butylene styrene based thermoplastic elastomers. Evoprene™ Super G has improved heat resistance and improved recovery properties over regular SEBS-based grades.
Can be used in food contact applications with the appropriate stabilizer package

Alphagary is part of Orbia.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.09 g/ccISO 2781
Viscosity Measurement 16
@Temperature 180 °C
Kg/cm2; Macklow-Smith extrusion rheometer
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 54ISO 868
Tensile Strength 7.70 MPaISO 37
Elongation at Break 575 %ISO 37
100% Modulus 0.00250 GPa
@Strain 100 %
ISO 37
Tear Strength 24.0 kN/mISO 34-B
Compression Set 14 %
@Temperature 22.0 °C,
Time 259000 sec
ISO 815
 21 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 33 %
@Temperature 100 °C,
Time 79200 sec
ISO 815
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 140 °C
Minimum Service Temperature, Air -60.0 °C
 
Descriptive Properties
Bonds withPolypropylene
 Polypropylene
 Polypropylene
Chemical ResistanceAcetoneGood
 Acids up to 80%Excellent
 AlcoholExcellent
 AlkalisExcellent
 Brake fluidGood
 Chlorinate solventsPoor
 DieselPoor
 Ethylene glycolExcellent
 GasolinePoor
 Salt solutionExcellent
 Soda lyeExcellent
 Water, 23°CExcellent
 Water, 95°CExcellent
TransparencyOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AlphaGary Evoprene™ COGEE 631 SEBS Thermoplastic Elastomer
AlphaGary Evoprene™ COGEE 637 SEBS Thermoplastic Elastomer
AlphaGary Evoprene™ G 3315 SEBS Thermoplastic Elastomer
AlphaGary Evoprene™ G 6087 SEBS Thermoplastic Elastomer
AlphaGary Evoprene™ G 614 SEBS Thermoplastic Elastomer

PGARY9744 / 140537

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.