MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales
metalmen Is Your Direct to US Manufacturing Source for High Purity Metals

(Viewing data as-entered. Click here to return)
Chromium, Cr; As-Swaged
Categories: Metal; Nonferrous Metal; Pure Element

Material Notes: As-swaged applies only to tensile and/or hardness values; other property values are typical of the element.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.19 g/cc
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 51.99611995
Atomic Number 24
Thermal Neutron Cross Section 2.9 barns/atom
X-ray Absorption Edge 2.07 ÅK
 18.256 ÅLI
 21.226 ÅLII
 21.5958 ÅLIII
Electrode Potential -0.560 V
Electronegativity 1.66Pauling
Ionic Radius 0.520 ÅCrystal Ionic Radius for Valence +6
 0.630 ÅCrystal Ionic Radius for Valence +3
 0.810 ÅCrystal Ionic Radius for Valence +1
 0.890 ÅCrystal Ionic Radius for Valence +2
Electrochemical Equivalent 0.971 g/A/h
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 125
Hardness, Knoop 144Converted from Brinell
Hardness, Rockwell B 72Converted from Brinell
Hardness, Vickers 131Converted from Brinell
Tensile Strength, Ultimate 413 MPa
Tensile Strength, Yield 362 MPa
Elongation at Break 44 %
Charpy Impact, Unnotched 2.00 JUnspecified Heat Treatment.
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 5.00e-7 ohm-cm
@Temperature -260 °C
 0.0000130 ohm-cm
@Temperature 20.0 °C
 0.0000180 ohm-cm
@Temperature 152 °C
 0.0000200 ohm-cm
@Temperature 200 °C
 0.0000310 ohm-cm
@Temperature 407 °C
 0.0000400 ohm-cm
@Temperature 600 °C
 0.0000470 ohm-cm
@Temperature 652 °C
 0.0000660 ohm-cm
@Temperature 1000 °C
Magnetic Susceptibility 0.0000035cgs/g
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 293.1 J/g
Heat of Vaporization 5945 J/g
CTE, linear 6.20 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.461 J/g-°C
Thermal Conductivity 69.1 W/m-K
Melting Point 1860 °C
Boiling Point 2671 °C
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.10
@Temperature 50.0 °C
polished, total radiation
Reflection Coefficient, Visible (0-1) 0.70500 nm
 
Component Elements PropertiesOriginal ValueComments
Chromium, Cr 100 %
 
Descriptive Properties
CAS Number7440-47-3

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chromium, Cr; Recrystallized
Chromium, Cr; Annealed
Special Metals INCONEL® Alloy 718
AISI 4140 Steel, normalized at 870°C (1600°F), air cooled, 100 mm (4 in.) round
AISI E4340 Steel, heat treated, fatigue tested

AMECr00 / 24

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.