MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ATI Allegheny Ludlum 310 Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Stainless Steel; T 300 Series Stainless Steel; T S30000 Series Stainless Steel

Material Notes: Comparable corrosion resistance, superior resistance to oxidation, and the retention of a larger fraction of room temperature strength than common austenitic alloys. Good creep deformation resistance.

Applications:Heat treatment industry-conveyor belts, rollers, burner parts, refractory supports, retorts linings, oven linings, fans, tube hangers, baskets, and trays. Chemical process industry- containers for hot concentrated acids, ammonia, and sulfur dioxide. Food processing industry- used in contact with hot acetic and citric acid.

Typical property data reported.

Key Words: UNS S31000
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.03 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 617 MPaASTM E8
 48.0 MPa
@Temperature 1093 °C
ASTM E8
 76.0 MPa
@Temperature 871 °C
ASTM E8
 209 MPa
@Temperature 816 °C
ASTM E8
 394 MPa
@Temperature 649 °C
ASTM E8
 483 MPa
@Temperature 538 °C
ASTM E8
 516 MPa
@Temperature 427 °C
ASTM E8
 528 MPa
@Temperature 204 °C
ASTM E8
Tensile Strength, Yield 136 MPa
@Temperature 816 °C
ASTM E8
 156 MPa
@Temperature 649 °C
ASTM E8
 167 MPa
@Temperature 538 °C
ASTM E8
 188 MPa
@Temperature 427 °C
ASTM E8
 217 MPa
@Temperature 204 °C
ASTM E8
 292 MPa
@Strain 0.2 %
ASTM E8
Elongation at Break 45 %ASTM E8
 36 %
@Temperature 538 °C
ASTM E8
 37 %
@Temperature 427 °C
ASTM E8
 37.5 %
@Temperature 204 °C
ASTM E8
 41.5 %
@Temperature 649 °C
ASTM E8
 65 %
@Temperature 871 °C
ASTM E8
 66 %
@Temperature 816 °C
ASTM E8
 77 %
@Temperature 1093 °C
ASTM E8
Creep Strength 20.0 MPa
@Temperature 788 °C,
Time 3.60e+7 sec
1% creep
 138 MPa
@Temperature 593 °C,
Time 3.60e+7 sec
1% creep
Rupture Strength 20.0 MPa
@Temperature 899 °C,
Time 3.60e+7 sec
 138 MPa
@Temperature 593 °C,
Time 3.60e+7 sec
Modulus of Elasticity 200 GPa
Poissons Ratio 0.30calculated
Shear Modulus 77.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000780 ohm-cm
@Temperature 20.0 °C
Magnetic Permeability 1.02at 200H
 
Thermal PropertiesOriginal ValueComments
CTE, linear 15.9 µm/m-°C
@Temperature 20.0 - 100 °C
 17.1 µm/m-°C
@Temperature 20.0 - 500 °C
 18.9 µm/m-°C
@Temperature 20.0 - 1000 °C
Specific Heat Capacity 0.502 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 13.8 W/m-K
@Temperature 20.0 - 100 °C
 18.7 W/m-K
@Temperature 20.0 - 500 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.250 %
Chromium, Cr 24 - 26 %
Iron, Fe 48 - 57 %As Remainder
Manganese, Mn <= 2.00 %
Nickel, Ni 19 - 22 %
Phosphorus, P <= 0.0450 %
Silicon, Si <= 1.50 %
Sulfur, S <= 0.0300 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
310 Stainless Steel, annealed sheet
ATI Allegheny Ludlum 310H Austenitic Stainless Steel
ATI Allegheny Ludlum 310S Austenitic Stainless Steel
310 Stainless Steel, annealed strip
Sandvik 310-7RE10 Billet

NL1004 / 17772

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.