MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LG Chemical AF342T ABS, Flame Retardant, High Impact  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Impact Grade, Molded

Material Notes: Feature: Injection Molding, Flame Retardant, High Impact

Application: Electric/Electronic Applications (TV, Monitor Housing) IT/OA device

CAS No. 9003-56-9, 40039-93-8 and 1309-64-4

Information provided by LG Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.18 g/ccASTM D792
Maximum Moisture Content 0.010Injection Molding
Linear Mold Shrinkage, Flow 0.0040 - 0.0070 cm/cm
@Thickness 3.20 mm
ASTM D955
Melt Flow 40 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 98ASTM D785
Tensile Strength, Yield 410 kg(f)/cm²
@Thickness 3.20 mm
50 mm/min; ASTM D638
Elongation at Break 20 %
@Thickness 3.20 mm
50 mm/min; ASTM D638
Elongation at Yield >= 5.0 %
@Thickness 3.20 mm
50 mm/min; ASTM D638
Tensile Modulus 22000 kg(f)/cm²
@Thickness 3.20 mm
1 mm/min; ASTM D638
Flexural Yield Strength 650 kg(f)/cm²
@Thickness 6.40 mm
15 mm/min; ASTM D790
Flexural Modulus 21500 kg(f)/cm²
@Thickness 6.40 mm
15 mm/min; ASTM D790
Izod Impact, Notched 21.0 kg-cm/cm
@Thickness 6.40 mm,
Temperature 23.0 °C
ASTM D256
 27.0 kg-cm/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
ASTM D256
Izod Impact, Unnotched 6.00 kg-cm/cm
@Thickness 6.40 mm,
Temperature -30.0 °C
ASTM D256
 7.00 kg-cm/cm
@Thickness 3.20 mm,
Temperature -30.0 °C
ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+12 ohm-cm
Dielectric Strength 36.0 kV/mm
Arc Resistance 0.00 - 60 secASTM D495
Comparative Tracking Index 400 - 600 V
Hot Wire Ignition, HWI 7.0 - 15 sec
@Thickness >=1.50 mm
 7.0 - 15 sec
@Thickness >=2.00 mm
 7.0 - 15 sec
@Thickness >=2.50 mm
 60 - 120 sec
@Thickness >=3.00 mm
High Amp Arc Ignition, HAI >= 120 arcs
@Thickness 1.50 mm
 >= 120 arcs
@Thickness 2.00 mm
 >= 120 arcs
@Thickness 2.50 mm
 >= 120 arcs
@Thickness 3.00 mm
High Voltage Arc-Tracking Rate, HVTR >= 150 mm/min
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 89.0 °C
@Thickness 6.40 mm
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 81.0 °C
@Thickness 6.40 mm
Unannealed; ASTM D648
Vicat Softening Point 88.0 °C
@Load 5.00 kg
50°C/h; ASTM D1525
UL RTI, Electrical 60.0 °C
@Thickness >=1.50 mm
UL 746B
 60.0 °C
@Thickness >=2.00 mm
 60.0 °C
@Thickness >=2.50 mm
 60.0 °C
@Thickness >=3.00 mm
UL RTI, Mechanical with Impact 60.0 °C
@Thickness >=1.50 mm
UL 746B
 60.0 °C
@Thickness >=2.00 mm
 60.0 °C
@Thickness >=2.50 mm
 60.0 °C
@Thickness >=3.00 mm
UL RTI, Mechanical without Impact 60.0 °C
@Thickness >=1.50 mm
UL 746B
 60.0 °C
@Thickness >=2.00 mm
 60.0 °C
@Thickness >=2.50 mm
 60.0 °C
@Thickness >=3.00 mm
Flammability, UL94 V-0
@Thickness >=1.50 mm
 V-0
@Thickness >=2.00 mm
 V-0
@Thickness >=2.50 mm
 V-0
@Thickness >=3.00 mm
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 170 - 190 °CInjection Molding
Middle Barrel Temperature 180 - 200 °CInjection Molding
Front Barrel Temperature 190 - 210 °CInjection Molding
Nozzle Temperature 200 - 230 °CInjection Molding
Melt Temperature 200 - 230 °CInjection Molding
Mold Temperature 40.0 - 60.0 °CInjection Molding
Drying Temperature 70.0 - 80.0 °CInjection Molding
Dry Time 2.00 - 4.00 hourInjection Molding
Back Pressure 0.490 - 0.981 MPaInjection Molding
Screw Speed 30 - 60 rpmInjection Molding

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LG Chemical BM662 ABS, Heat Resistance
Cheng Yu Plastic VH823 Flame Retardant ABS, High Impact
Cheng Yu Plastic VH825 Flame Retardant ABS, Medium Impact
Cheng Yu Plastic VH826 Flame Retardant ABS, Medium Impact
LG Chemical 92HR SAN Resin

PLAY083 / 148091

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.