MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
TSE Industries Millathane® CM Millable Polyether Urethane Rubber with 10 PHR N774 Filler
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Elastomer, Unreinforced; Rubber or Thermoset Elastomer (TSE)

Material Notes: MILLATHANE CM is a sulfur and peroxide curable polyether urethane rubber. Its outstanding property is its great resistance to abrasion, which makes it of special interest for articles that are subjected to high wear in service. It has a unique combination of excellent properties, such as low temperature characteristics, and resistance to heat deterioration, ozone cracking, weathering and swelling in oils or solvents.

All information provided by TSE Industries

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.12 g/cc
Mooney Viscosity 21
@Temperature 121 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 56
Tensile Strength 3900 psi
Elongation at Break 580 %
100% Modulus 0.200 ksi
@Strain 100 %
300% Modulus 0.750 ksi
@Strain 300 %
Tear Strength 37.8 kN/mGraves
Abrasion 100NBS Index
Compression Set 25 %Method B
 
Processing PropertiesOriginal ValueComments
Cure Time 60.0 min
@Temperature 142 °C
 
Descriptive Properties
Formulation as Tested0.35CAYTUR 4
 0.5Zinc Stearate
 0.75Sulfur
 1MBT
 10N774
 100Millathane CM
 3.33Coumarone-Indene Resin
 4MBTS

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polycarbonate-Urethane
Mearthane Durethane™ C 10-30A Polyurethane
TSE Industries Millathane® CM Millable Polyether Urethane Rubber with 1-D Heavy Oil Plasticizer
TSE Industries Millathane® CM Millable Polyether Urethane Rubber with 45 PHR N990 Filler
TSE Industries Millathane® CM Millable Polyether Urethane Rubber, 0.20 PHR Caytur 4

PMILL172 / 87216

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.