MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Delrin Delrin® 127UV BK701 POM
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: UV Stabilized High Viscosity Acetal Homopolymer

Information provided by DuPont; Delrin was sold by DuPont in 2023.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.42 g/ccISO 1183
Melt Flow 2.5 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 71.5 MPaISO 527-1/-2
Elongation at Break 37 %Nominal; ISO 527-1/-2
Elongation at Yield 22 %ISO 527-1/-2
Tensile Modulus 3000 MPaISO 527-1/-2
Flexural Modulus 2800 MPaISO 178
Poissons Ratio 0.37
Charpy Impact, Notched 10.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 13.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 110 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°CISO 11359-1/-2
Melting Point 178 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 162 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 92.0 °CISO 75-1/-2
Flammability, UL94 HB
@Thickness 0.800 mm
IEC 60695-11-10
Flame Spread 26.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
 
Processing PropertiesOriginal ValueComments
Melt Temperature 195 - 205 °CRange, Extrusion
 200 °COptimum, Extrusion
 215 °COptimum, Injection
 210 - 220 °CRange, Injection
Mold Temperature 90.0 °COptimum, Injection
 80.0 - 100 °CInjection
Drying Temperature 80.0 °CInjection
 80.0 °CExtrusion
Dry Time 2.00 - 4.00 hourExtrusion, Dehumidified Dryer
 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %Extrusion
 <= 0.20 %Injection
Hold Pressure 90.0 - 110 MPaInjection
 110 MPaInjection
Annealing Temperature 160 °COptional; 2 mm/min; Injection
 
Descriptive Properties
AdditivesRelease agent
Annealing time (min/mm)30Optional, Injection
Drying RecommendedyesInjection
Emissions (mg/kg)<8VDA 275
FMVSS ClassBISO 3795 (FMVSS 302)
Max. screw tangential speed (m/s)0.2Injection
Part Marking Code>POM<ISO 11469
PolymerPOM
Processing Hold Pressure Time (s/mm)8Injection
Resin IdentificationPOMISO 1043
Weather stability delta E0.4DIN 53236
Weather stability grey scale4 to 5ISO 105-A02

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Delrin Delrin® 127UV NC010 POM
Delrin Delrin® 527UV NC010 POM
DuPont Mobility and Materials Delrin® 127UVE RD402 POM
Delrin Delrin® 127UVE NC010 POM
DuPont Mobility and Materials Delrin® 127UVE BK701 POM

PDSX5097 / 197737

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.