MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Industeel CLC 1.2316S Prehardened Mold Steel (300HB) with Improved Machinability
Categories: Metal; Ferrous Metal; Tool Steel; Mold Steel

Material Notes: Description: CLC 1.2316 S grade is a 16%Cr 1%Mo mold steel with improved corrosion resistance properties, thanks to the chromium and molybdenum additions. Furthermore specific sulfur additions are considered to increase the machinability properties. The grade in the quenched tempered condition has a fully bainite martensite microstructure and can be delivered in the prehardened condition (300HB or 340HB). The grade is not designed for highly finish polished surfaces or etched surfaces. The grade is commonly used for mold steel applications including cores, inserts, molds… subjected to wet working conditions and / or storage conditions. The grade is also used for the manufacturing of corrosive materials like PVC.

Information provided by manufacturer.

Key Words: AFNOR Z40CD16 (S), DIN X36CrMo17 (S) - X33CrS16, WERKSTOFF Nbr 1.2316 with S addition - (» 1.2085)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.75 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 340Typical, in Longitudinal
Tensile Strength, Ultimate 1160 MPaTypical, Longitudinal Direction
Tensile Strength, Yield 950 MPa
@Strain 0.2 %
Typical, Longitudinal Direction
Elongation at Break 10 %Typical, EL 5.65 Longitudinal Direction
Modulus of Elasticity 207 GPaTypical, in Longitudinal Direction
Charpy Impact 12.0 JTypical (Longitudinal)
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.0 µm/m-°C
@Temperature 20.0 - 100 °C
 11.1 µm/m-°C
@Temperature 20.0 - 200 °C
 11.7 µm/m-°C
@Temperature 20.0 - 400 °C
Specific Heat Capacity 0.460 J/g-°C
@Temperature 20.0 °C
Thermal Conductivity 24.3 W/m-K
@Temperature 20.0 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.40 %
Chromium, Cr 16 %
Iron, Fe 81.32 - 81.42 %As remainder
Manganese, Mn 0.80 %
Molybdenum, Mo 1.03 %
Phosphorus, P <= 0.030 %
Silicon, Si 0.35 %
Sulfur, S <= 0.070 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Industeel CLC 1.2316 Prehardened (300HB) and Corrosion Resistant Mold Steel
Bohler-Uddeholm M300 Modified 420
Bohler-Uddeholm BÖHLER W400 VMR® H11 Hot Work Tool Steel
17-7 PH Stainless Steel, CH900, plate, sheet, and strip
ASTM A284 Steel, grade C

NINDUST52 / 17590

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.