MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Carpenter Chrome Core® 8-FM Alloy
Categories: Metal; Electronic/Magnetic Alloy; Ferrous Metal

Material Notes: Data provided by Carpenter Technology Corporation.

Chrome Core® alloys are a family of controlled chemistry, ferritic 8 and 12% chromium-iron alloys which are candidates for use in magnetic components where corrosion resistance superior to that of pure iron, low carbon steel and silicon-iron alloys is desired without the substantial decrease in saturation induction associated with the 18% Cr ferritic stainless steels.

Applications could include electro-mechanical devices requiring some degree of corrosion resistance, either in service or for extended shelf life without the need for protective coatings. Chrome Core alloys have been considered for use in automotive components such as fuel injectors, fuel pump motor laminations and ABS solenoids. Each chrome level is available in both a standard and a free-machining grade.

Chrome Core® is a registered trademark of Carpenter Technology Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.70 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 73
Tensile Strength, Ultimate 421 MPa
Tensile Strength, Yield 228 MPa
@Strain 0.2 %
Elongation at Break 50 %in 50 mm
Reduction of Area 73 %
Modulus of Elasticity 200 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000490 ohm-cm
Curie Temperature 750 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.2 µm/m-°C
@Temperature 25.0 - 50.0 °C
 11.6 µm/m-°C
@Temperature 25.0 - 300 °C
 12.6 µm/m-°C
@Temperature 25.0 - 600 °C
Specific Heat Capacity 0.415 J/g-°C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.030 %
Chromium, Cr 7.5 - 8.5 %
Iron, Fe 90 %as remainder
Manganese, Mn 0.20 - 0.70 %
Molybdenum, Mo 0.20 - 0.50 %
Phosphorus, P 0.030 %
Silicon, Si 0.30 - 0.70 %
Sulfur, S 0.20 - 0.40 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Carpenter Chrome Core® 8 Alloy
Carpenter Chrome Core® 12 Alloy
Carpenter Chrome Core® 12-FM Alloy
Iron (II) Hydroxide, Fe(OH)2
Crucible Steel PDCQ Premium Quality High Toughness H13 Steel

NCARG1 / 15762

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.