MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Erbslöh Aluminium DISPAL S263 Aluminum Alloy, AlSi25Cu3Fe3Ni3MgCoTi, Condition T4
Categories: Metal; Nonferrous Metal; Aluminum Alloy

Material Notes: Excellent properties:
  • abrasive stability
  • high stiffness (E-modulus)
  • resistance even at high temperatures
  • good grindability

PEAK DISPAL materials allow the manufacturing of pistons for highest operational demands.

Property data for Heat Treatment Condition T4 (Quenching in water at RT).

Information provided by PEAK Werkstoff GmbH, a part of Erbslöh Aluminium GmbH.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.622 - 2.898 g/cc0.09473 - 0.1047 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers >= 190>= 190HV30
Tensile Strength at Break >= 464 MPa
@Temperature 20.0 °C
>= 67300 psi
@Temperature 68.0 °F
Tensile Strength, Yield >= 355 MPa
@Temperature 20.0 °C
>= 51500 psi
@Temperature 68.0 °F
Elongation at Break >= 0.60 %
@Temperature 20.0 °C
>= 0.60 %
@Temperature 68.0 °F
Modulus of Elasticity  >= 73.0 GPa
@Temperature 300 °C
>= 10600 ksi
@Temperature 572 °F
Condition T6
 >= 81.0 GPa
@Temperature 250 °C
>= 11700 ksi
@Temperature 482 °F
Condition T6
 >= 96.0 GPa
@Temperature 20.0 °C
>= 13900 ksi
@Temperature 68.0 °F
Poissons Ratio  0.286
@Temperature 20.0 °C
0.286
@Temperature 68.0 °F
Condition F
 0.289
@Temperature 100 °C
0.289
@Temperature 212 °F
Condition F
 0.29
@Temperature 150 °C
0.29
@Temperature 302 °F
Condition F
 0.291
@Temperature 200 °C
0.291
@Temperature 392 °F
Condition F
 0.294
@Temperature 250 °C
0.294
@Temperature 482 °F
Condition F
 0.294
@Temperature 300 °C
0.294
@Temperature 572 °F
Condition F
Fatigue Strength 206.5 MPa
@Temperature 20.0 °C
29950 psi
@Temperature 68.0 °F
P50% rotary bending values for 5X107 cycles
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000910 - 0.0000100 ohm-cm0.00000910 - 0.0000100 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  15.3 - 16.3 µm/m-°C
@Temperature 20.0 - 100 °C
8.50 - 9.06 µin/in-°F
@Temperature 68.0 - 212 °F
 16.1 - 17.1 µm/m-°C
@Temperature 20.0 - 200 °C
8.94 - 9.50 µin/in-°F
@Temperature 68.0 - 392 °F
 17.0 - 18.0 µm/m-°C
@Temperature 20.0 - 300 °C
9.44 - 10.0 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.840 - 0.880 J/g-°C0.201 - 0.210 BTU/lb-°F
Thermal Conductivity  95.30 W/m-K
@Temperature 400 °C
661.4 BTU-in/hr-ft²-°F
@Temperature 752 °F
 99.20 W/m-K
@Temperature 200 °C
688.4 BTU-in/hr-ft²-°F
@Temperature 392 °F
 99.20 W/m-K
@Temperature 300 °C
688.4 BTU-in/hr-ft²-°F
@Temperature 572 °F
 99.60 W/m-K
@Temperature 100 °C
691.2 BTU-in/hr-ft²-°F
@Temperature 212 °F
 101.2 W/m-K
@Temperature 30.0 °C
702.3 BTU-in/hr-ft²-°F
@Temperature 86.0 °F
Melting Point 528 - 784 °C982 - 1440 °F
Solidus 528.1 - 534.1 °C982.6 - 993.4 °F
Liquidus 784.2 - 790.2 °C1444 - 1454 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 63 %63 %As Balance
Cobalt, Co 1.0 %1.0 %
Copper, Cu 3.0 %3.0 %
Iron, Fe 3.0 %3.0 %
Magnesium, Mg 1.0 %1.0 %
Nickel, Ni 3.0 %3.0 %
Silicon, Si 25 %25 %
Titanium, Ti 1.0 %1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Erbslöh Aluminium DISPAL S220 Aluminum Alloy, AlSi35, Condition O
Erbslöh Aluminium DISPAL S693 Aluminum Alloy, AlCu5Ti, Condition T6
Erbslöh Aluminium DISPAL S226 Aluminum Alloy, AlSi30CuMg, Condition T6
Erbslöh Aluminium DISPAL S236 Aluminum Alloy, Condition T6(SB)
Erbslöh Aluminium DISPAL S260 Aluminum Alloy, AlSi25Cu4Mg, Condition T6

NPEAK06ay / 170262

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.