  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Mocom (ALBIS) ALCOM® LB PP 4040 LE 15085 WT1132-15 PP, 40% Mineral Reinforced
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Mineral Reinforced

Material Notes: Base Polymer: Polypropylene Homopolymer

Filler/Additive System: 40% mineral

Special Features: Highly reflective, opaque, low emission

Market Segment: Automotive, Lighting

Application Area: Lighting, light blocking components

Typical Application: Light guides, reflectors

Information provided by Albis Plastics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.30 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.010 - 0.012 cm/cm
@Time 86400 sec
ISO 294-4
Linear Mold Shrinkage, Transverse 0.0080 - 0.010 cm/cm
@Time 86400 sec
ISO 294-4
Melt Flow 24 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 32.0 MPaISO 527
Elongation at Break 4.1 %ISO 527
Elongation at Yield 2.1 %ISO 527
Tensile Modulus 4200 MPaISO 527
Flexural Strength 53.0 MPaISO 178
Flexural Modulus 4200 MPaISO 178
Charpy Impact Unnotched 10.0 kJ/m²
@Temperature -40.0 °C
ISO 179/1eU
 25.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 1.50 kJ/m²
@Temperature -40.0 °C
ISO 179/1eA
 2.00 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 94.0 °CISO 75-1/-2
Vicat Softening Point 110 °CB50; ISO 306
 
Optical PropertiesOriginal ValueComments
Transmission, Visible 0.10 %
@Thickness 0.500 mm
ISO 13468
Reflection Coefficient, Visible (0-1) 0.94DIN 5033
 
Processing PropertiesOriginal ValueComments
Melt Temperature 200 - 270 °CInjection molding
Mold Temperature 20.0 - 90.0 °CInjection molding
Drying Temperature 80.0 - 100 °C
@Time 7200 - 10800 sec
in a dry air (desiccant) dryer
 80.0 - 100 °C
@Time 7200 - 14400 sec
in an circulating dryer
 
Descriptive Properties
Base PolymerPolypropylene Homopolymer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Plastcom SLOVALEN PH 78 T 40 PP, 40% mineral filling
Plastcom SLOVALEN PH 71 T 40 PP, 40% mineral filling
Plastcom SLOVALEN PH 72 T 40 PP, 40% mineral filling
Plastcom SLOVALEN PC 92 T 40 PP, 40% mineral filling
Plastcom SLOVALEN PC 51 T 40 PP, 40% mineral filling

PALBIS8462 / 242521

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.